Description

The austenitic material X2CrNiMo17-12-3 is used in solution annealed condition in the form of cold rolled strip, warm rolled strip and warm rolled sheet as well as in the form of rods, wire rod and profiles. It is resistant to intercrystalline corrosion also in sensitized condition.

Related Standards

Equivalent Materials

This material data has been provided by WIAM.

All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

Ashby charts

See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Properties

General

PropertyTemperatureValue

Density

20.0 °C

8 g/cm³

Show Material materials with Density of 8 g/cm³

Mechanical

PropertyTemperatureValueComment

Elastic modulus

20.0 °C

200 GPa

Show Material materials with Elastic modulus of 200 GPa

100.0 °C

194 GPa

Show Material materials with Elastic modulus of 194 GPa

200.0 °C

186 GPa

Show Material materials with Elastic modulus of 186 GPa

300.0 °C

179 GPa

Show Material materials with Elastic modulus of 179 GPa

400.0 °C

172 GPa

Show Material materials with Elastic modulus of 172 GPa

500.0 °C

165 GPa

Show Material materials with Elastic modulus of 165 GPa

Elongation

20.0 °C

20 - 40 %

Show Material materials with Elongation of 20 - 40 %

Elongation A80, transverse

20.0 °C

40 - 45 %

Show Material materials with Elongation A80, transverse of 40 - 45 %

Elongation, transverse

20.0 °C

30 - 45 %

Show Material materials with Elongation, transverse of 30 - 45 %

Hardness, Brinell

20.0 °C

215 [-]

Show Material materials with Hardness, Brinell of 215 [-]

Hardness, Brinell, trans

20.0 °C

215 [-]

Show Material materials with Hardness, Brinell, trans of 215 [-]

Poisson's ratio

23.0 °C

0.3 [-]

Show Material materials with Poisson's ratio of 0.3 [-]

Typical for Austenitic Stainless Steel

Shear modulus

23.0 °C

77 GPa

Show Material materials with Shear modulus of 77 GPa

Typical for Austenitic Stainless Steel

Tensile strength

20.0 °C

500 - 1100 MPa

Show Material materials with Tensile strength of 500 - 1100 MPa

Tensile strength, transverse

20.0 °C

500 - 700 MPa

Show Material materials with Tensile strength, transverse of 500 - 700 MPa

Yield strength Rp0.2

20.0 °C

200 - 400 MPa

Show Material materials with Yield strength Rp0.2 of 200 - 400 MPa

100.0 °C

165 - 166 MPa

Show Material materials with Yield strength Rp0.2 of 165 - 166 MPa

150.0 °C

150 - 152 MPa

Show Material materials with Yield strength Rp0.2 of 150 - 152 MPa

200.0 °C

137 MPa

Show Material materials with Yield strength Rp0.2 of 137 MPa

250.0 °C

127 MPa

Show Material materials with Yield strength Rp0.2 of 127 MPa

300.0 °C

118 - 119 MPa

Show Material materials with Yield strength Rp0.2 of 118 - 119 MPa

350.0 °C

113 MPa

Show Material materials with Yield strength Rp0.2 of 113 MPa

400.0 °C

108 MPa

Show Material materials with Yield strength Rp0.2 of 108 MPa

450.0 °C

103 MPa

Show Material materials with Yield strength Rp0.2 of 103 MPa

500.0 °C

100 MPa

Show Material materials with Yield strength Rp0.2 of 100 MPa

550.0 °C

98 MPa

Show Material materials with Yield strength Rp0.2 of 98 MPa

Unlock all property charts

Yield strength Rp0.2, transverse

20.0 °C

200 - 240 MPa

Show Material materials with Yield strength Rp0.2, transverse of 200 - 240 MPa

Yield strength Rp1.0

20.0 °C

235 MPa

Show Material materials with Yield strength Rp1.0 of 235 MPa

100.0 °C

199 - 200 MPa

Show Material materials with Yield strength Rp1.0 of 199 - 200 MPa

150.0 °C

180 - 181 MPa

Show Material materials with Yield strength Rp1.0 of 180 - 181 MPa

200.0 °C

165 - 167 MPa

Show Material materials with Yield strength Rp1.0 of 165 - 167 MPa

250.0 °C

153 - 157 MPa

Show Material materials with Yield strength Rp1.0 of 153 - 157 MPa

300.0 °C

145 MPa

Show Material materials with Yield strength Rp1.0 of 145 MPa

350.0 °C

139 MPa

Show Material materials with Yield strength Rp1.0 of 139 MPa

400.0 °C

135 MPa

Show Material materials with Yield strength Rp1.0 of 135 MPa

450.0 °C

130 MPa

Show Material materials with Yield strength Rp1.0 of 130 MPa

500.0 °C

128 MPa

Show Material materials with Yield strength Rp1.0 of 128 MPa

550.0 °C

127 MPa

Show Material materials with Yield strength Rp1.0 of 127 MPa

Unlock all property charts

Yield strength Rp1.0, transverse

20.0 °C

235 - 270 MPa

Show Material materials with Yield strength Rp1.0, transverse of 235 - 270 MPa

Thermal

PropertyTemperatureValueComment

Coefficient of thermal expansion

100.0 °C

1.6E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.6E-5 1/K

200.0 °C

1.65E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.65E-5 1/K

300.0 °C

1.7E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.7E-5 1/K

400.0 °C

1.75E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.75E-5 1/K

500.0 °C

1.8E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.8E-5 1/K

Unlock all property charts

Melting point

1230 - 1480 °C

Show Material materials with Melting point of 1230 - 1480 °C

Typical for Austenitic Stainless Steel

Specific heat capacity

20.0 °C

500 J/(kg·K)

Show Material materials with Specific heat capacity of 500 J/(kg·K)

Thermal conductivity

20.0 °C

15 W/(m·K)

Show Material materials with Thermal conductivity of 15 W/(m·K)

Electrical

PropertyTemperatureValue

Electrical resistivity

20.0 °C

7.5E-7 Ω·m

Show Material materials with Electrical resistivity of 7.5E-7 Ω·m

Chemical properties

PropertyValue

Carbon

0.03 %

Show Material materials with Carbon of 0.03 %

Chromium

16.5 - 18.5 %

Show Material materials with Chromium of 16.5 - 18.5 %

Manganese

2 %

Show Material materials with Manganese of 2 %

Molybdenum

2.5 - 3 %

Show Material materials with Molybdenum of 2.5 - 3 %

Nickel

10.5 - 13 %

Show Material materials with Nickel of 10.5 - 13 %

Nitrogen

0.11 %

Show Material materials with Nitrogen of 0.11 %

Phosphorus

0.05 %

Show Material materials with Phosphorus of 0.05 %

Silicon

1 %

Show Material materials with Silicon of 1 %

Sulfur

0.015 %

Show Material materials with Sulfur of 0.015 %