General
Property | Temperature | Value |
---|---|---|
Density | 20.0 °C | 7.92 g/cm³ Show Material materials with Density of 7.92 g/cm³ |
Mechanical
Property | Temperature | Value |
---|---|---|
Elastic modulus | -100.0 °C | 206 GPa Show Material materials with Elastic modulus of 206 GPa |
20.0 °C | 196 GPa Show Material materials with Elastic modulus of 196 GPa | |
100.0 °C | 190 GPa Show Material materials with Elastic modulus of 190 GPa | |
200.0 °C | 182 GPa Show Material materials with Elastic modulus of 182 GPa | |
300.0 °C | 174 GPa Show Material materials with Elastic modulus of 174 GPa | |
400.0 °C | 166 GPa Show Material materials with Elastic modulus of 166 GPa | |
500.0 °C | 158 GPa Show Material materials with Elastic modulus of 158 GPa | |
600.0 °C | 150 GPa Show Material materials with Elastic modulus of 150 GPa | |
700.0 °C | 142 GPa Show Material materials with Elastic modulus of 142 GPa | |
800.0 °C | 134 GPa Show Material materials with Elastic modulus of 134 GPa | |
Poisson's ratio | 20.0 °C | 0.28 [-] Show Material materials with Poisson's ratio of 0.28 [-] |
Reduction of area | 20.0 °C | 40 % Show Material materials with Reduction of area of 40 % |
Tensile strength | 20.0 °C | 800 - 1000 MPa Show Material materials with Tensile strength of 800 - 1000 MPa |
Thermal
Property | Temperature | Value |
---|---|---|
Coefficient of thermal expansion | -100.0 °C | 1.49E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.49E-5 1/K |
20.0 °C | 1.61E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.61E-5 1/K | |
100.0 °C | 1.67E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.67E-5 1/K | |
200.0 °C | 1.72E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.72E-5 1/K | |
300.0 °C | 1.77E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.77E-5 1/K | |
400.0 °C | 1.81E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.81E-5 1/K | |
500.0 °C | 1.84E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.84E-5 1/K | |
600.0 °C | 1.88E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.88E-5 1/K | |
700.0 °C | 1.91E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.91E-5 1/K | |
800.0 °C | 1.94E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.94E-5 1/K | |
Max service temperature, long | -150 - 350 °C Show Material materials with Max service temperature, long of -150 - 350 °C | |
Specific heat capacity | -100.0 °C | 440 J/(kg·K) Show Material materials with Specific heat capacity of 440 J/(kg·K) |
20.0 °C | 472 J/(kg·K) Show Material materials with Specific heat capacity of 472 J/(kg·K) | |
100.0 °C | 487 J/(kg·K) Show Material materials with Specific heat capacity of 487 J/(kg·K) | |
200.0 °C | 503 J/(kg·K) Show Material materials with Specific heat capacity of 503 J/(kg·K) | |
300.0 °C | 512 J/(kg·K) Show Material materials with Specific heat capacity of 512 J/(kg·K) | |
400.0 °C | 520 J/(kg·K) Show Material materials with Specific heat capacity of 520 J/(kg·K) | |
500.0 °C | 530 J/(kg·K) Show Material materials with Specific heat capacity of 530 J/(kg·K) | |
600.0 °C | 541 J/(kg·K) Show Material materials with Specific heat capacity of 541 J/(kg·K) | |
700.0 °C | 551 J/(kg·K) Show Material materials with Specific heat capacity of 551 J/(kg·K) | |
800.0 °C | 559 J/(kg·K) Show Material materials with Specific heat capacity of 559 J/(kg·K) | |
Thermal conductivity | -100.0 °C | 11.7 W/(m·K) Show Material materials with Thermal conductivity of 11.7 W/(m·K) |
20.0 °C | 14.5 W/(m·K) Show Material materials with Thermal conductivity of 14.5 W/(m·K) | |
100.0 °C | 16 W/(m·K) Show Material materials with Thermal conductivity of 16 W/(m·K) | |
200.0 °C | 17.6 W/(m·K) Show Material materials with Thermal conductivity of 17.6 W/(m·K) | |
300.0 °C | 19.1 W/(m·K) Show Material materials with Thermal conductivity of 19.1 W/(m·K) | |
400.0 °C | 20.4 W/(m·K) Show Material materials with Thermal conductivity of 20.4 W/(m·K) | |
500.0 °C | 21.9 W/(m·K) Show Material materials with Thermal conductivity of 21.9 W/(m·K) | |
600.0 °C | 23.3 W/(m·K) Show Material materials with Thermal conductivity of 23.3 W/(m·K) | |
700.0 °C | 24.7 W/(m·K) Show Material materials with Thermal conductivity of 24.7 W/(m·K) | |
800.0 °C | 26.1 W/(m·K) Show Material materials with Thermal conductivity of 26.1 W/(m·K) | |
Thermal diffusivity | -100.0 °C | 3.7 mm²/s Show Material materials with Thermal diffusivity of 3.7 mm²/s |
20.0 °C | 3.9 mm²/s Show Material materials with Thermal diffusivity of 3.9 mm²/s | |
100.0 °C | 4.3 mm²/s Show Material materials with Thermal diffusivity of 4.3 mm²/s | |
200.0 °C | 4.3 mm²/s Show Material materials with Thermal diffusivity of 4.3 mm²/s | |
300.0 °C | 4.6 mm²/s Show Material materials with Thermal diffusivity of 4.6 mm²/s | |
400.0 °C | 4.7 mm²/s Show Material materials with Thermal diffusivity of 4.7 mm²/s | |
500.0 °C | 4.9 mm²/s Show Material materials with Thermal diffusivity of 4.9 mm²/s | |
600.0 °C | 5 mm²/s Show Material materials with Thermal diffusivity of 5 mm²/s | |
700.0 °C | 5.3 mm²/s Show Material materials with Thermal diffusivity of 5.3 mm²/s | |
800.0 °C | 5.7 mm²/s Show Material materials with Thermal diffusivity of 5.7 mm²/s | |
Electrical
Property | Temperature | Value |
---|---|---|
Electrical resistivity | -100.0 °C | 5.86E-7 Ω·m Show Material materials with Electrical resistivity of 5.86E-7 Ω·m |
20.0 °C | 6.92E-7 Ω·m Show Material materials with Electrical resistivity of 6.92E-7 Ω·m | |
100.0 °C | 7.58E-7 Ω·m Show Material materials with Electrical resistivity of 7.58E-7 Ω·m | |
200.0 °C | 8.36E-7 Ω·m Show Material materials with Electrical resistivity of 8.36E-7 Ω·m | |
300.0 °C | 9.07E-7 Ω·m Show Material materials with Electrical resistivity of 9.07E-7 Ω·m | |
400.0 °C | 9.73E-7 Ω·m Show Material materials with Electrical resistivity of 9.73E-7 Ω·m | |
500.0 °C | 1.02E-6 Ω·m Show Material materials with Electrical resistivity of 1.02E-6 Ω·m | |
600.0 °C | 1.06E-6 Ω·m Show Material materials with Electrical resistivity of 1.06E-6 Ω·m | |
700.0 °C | 1.1E-6 Ω·m Show Material materials with Electrical resistivity of 1.1E-6 Ω·m | |
800.0 °C | 1.13E-6 Ω·m Show Material materials with Electrical resistivity of 1.13E-6 Ω·m | |
Chemical properties
Property | Value |
---|---|
Aluminium | 0.75 - 1.5 % Show Material materials with Aluminium of 0.75 - 1.5 % |
Carbon | 0.09 % Show Material materials with Carbon of 0.09 % |
Chromium | 16 - 18 % Show Material materials with Chromium of 16 - 18 % |
Manganese | 1 % Show Material materials with Manganese of 1 % |
Nickel | 6.5 - 7.75 % Show Material materials with Nickel of 6.5 - 7.75 % |
Phosphorus | 0.05 % Show Material materials with Phosphorus of 0.05 % |
Silicon | 1 % Show Material materials with Silicon of 1 % |
Sulfur | 0.03 % Show Material materials with Sulfur of 0.03 % |
Technological properties
Property | ||
---|---|---|
Features | Spring |