General
Property | Temperature | Value |
---|---|---|
Density | 20.0 °C | 7.73 g/cm³ Show Material materials with Density of 7.73 g/cm³ |
Mechanical
Property | Temperature | Value | Comment |
---|---|---|---|
Elastic modulus | 20.0 °C | 217 GPa Show Material materials with Elastic modulus of 217 GPa | |
100.0 °C | 215 GPa Show Material materials with Elastic modulus of 215 GPa | ||
200.0 °C | 188 GPa Show Material materials with Elastic modulus of 188 GPa | ||
300.0 °C | 164 GPa Show Material materials with Elastic modulus of 164 GPa | ||
Elongation | 20.0 °C | 20 % Show Material materials with Elongation of 20 % | |
Elongation, transverse | 20.0 °C | 18 % Show Material materials with Elongation, transverse of 18 % | |
Hardness, Brinell | 20.0 °C | 175 [-] Show Material materials with Hardness, Brinell of 175 [-] | |
Hardness, Vickers | 20.0 °C | 175 [-] Show Material materials with Hardness, Vickers of 175 [-] | |
Poisson's ratio | 23.0 °C | 0.3 [-] Show Material materials with Poisson's ratio of 0.3 [-] | Typical for Ferritic Stainless Steel |
Shear modulus | 23.0 °C | 77 GPa Show Material materials with Shear modulus of 77 GPa | Typical for Ferritic Stainless Steel |
Tensile strength | 20.0 °C | 390 - 560 MPa Show Material materials with Tensile strength of 390 - 560 MPa | |
Tensile strength, transverse | 20.0 °C | 390 - 560 MPa Show Material materials with Tensile strength, transverse of 390 - 560 MPa | |
Yield strength | 20.0 °C | 190 MPa Show Material materials with Yield strength of 190 MPa | |
Yield strength, transverse | 20.0 °C | 190 MPa Show Material materials with Yield strength, transverse of 190 MPa |
Thermal
Property | Temperature | Value | Comment |
---|---|---|---|
Coefficient of thermal expansion | 20.0 °C | 1.02E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.02E-5 1/K | |
100.0 °C | 1.05E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.05E-5 1/K | ||
200.0 °C | 1.09E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.09E-5 1/K | ||
300.0 °C | 1.13E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.13E-5 1/K | ||
400.0 °C | 1.16E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.16E-5 1/K | ||
500.0 °C | 1.2E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.2E-5 1/K | ||
600.0 °C | 1.22E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.22E-5 1/K | ||
Melting point | 1425 - 1530 °C Show Material materials with Melting point of 1425 - 1530 °C | Typical for Ferritic Stainless Steel | |
Specific heat capacity | 20.0 °C | 439 J/(kg·K) Show Material materials with Specific heat capacity of 439 J/(kg·K) | |
100.0 °C | 474 J/(kg·K) Show Material materials with Specific heat capacity of 474 J/(kg·K) | ||
200.0 °C | 498 J/(kg·K) Show Material materials with Specific heat capacity of 498 J/(kg·K) | ||
300.0 °C | 517 J/(kg·K) Show Material materials with Specific heat capacity of 517 J/(kg·K) | ||
400.0 °C | 538 J/(kg·K) Show Material materials with Specific heat capacity of 538 J/(kg·K) | ||
500.0 °C | 564 J/(kg·K) Show Material materials with Specific heat capacity of 564 J/(kg·K) | ||
600.0 °C | 598 J/(kg·K) Show Material materials with Specific heat capacity of 598 J/(kg·K) | ||
Thermal conductivity | 20.0 °C | 25.9 W/(m·K) Show Material materials with Thermal conductivity of 25.9 W/(m·K) | |
100.0 °C | 25.3 W/(m·K) Show Material materials with Thermal conductivity of 25.3 W/(m·K) | ||
200.0 °C | 25.2 W/(m·K) Show Material materials with Thermal conductivity of 25.2 W/(m·K) | ||
300.0 °C | 25.2 W/(m·K) Show Material materials with Thermal conductivity of 25.2 W/(m·K) | ||
400.0 °C | 25.4 W/(m·K) Show Material materials with Thermal conductivity of 25.4 W/(m·K) | ||
500.0 °C | 25.7 W/(m·K) Show Material materials with Thermal conductivity of 25.7 W/(m·K) | ||
600.0 °C | 25.9 W/(m·K) Show Material materials with Thermal conductivity of 25.9 W/(m·K) | ||
Thermal diffusivity | 20.0 °C | 7.6 mm²/s Show Material materials with Thermal diffusivity of 7.6 mm²/s | |
100.0 °C | 6.6 mm²/s Show Material materials with Thermal diffusivity of 6.6 mm²/s | ||
200.0 °C | 6.1 mm²/s Show Material materials with Thermal diffusivity of 6.1 mm²/s | ||
300.0 °C | 5.8 mm²/s Show Material materials with Thermal diffusivity of 5.8 mm²/s | ||
400.0 °C | 5.3 mm²/s Show Material materials with Thermal diffusivity of 5.3 mm²/s | ||
500.0 °C | 4.8 mm²/s Show Material materials with Thermal diffusivity of 4.8 mm²/s | ||
600.0 °C | 4.1 mm²/s Show Material materials with Thermal diffusivity of 4.1 mm²/s | ||
Electrical
Property | Temperature | Value |
---|---|---|
Electrical resistivity | 20.0 °C | 5.59E-7 Ω·m Show Material materials with Electrical resistivity of 5.59E-7 Ω·m |
100.0 °C | 6.4E-7 Ω·m Show Material materials with Electrical resistivity of 6.4E-7 Ω·m | |
200.0 °C | 7.32E-7 Ω·m Show Material materials with Electrical resistivity of 7.32E-7 Ω·m | |
300.0 °C | 8.17E-7 Ω·m Show Material materials with Electrical resistivity of 8.17E-7 Ω·m | |
400.0 °C | 8.97E-7 Ω·m Show Material materials with Electrical resistivity of 8.97E-7 Ω·m | |
500.0 °C | 9.74E-7 Ω·m Show Material materials with Electrical resistivity of 9.74E-7 Ω·m | |
600.0 °C | 1.05E-6 Ω·m Show Material materials with Electrical resistivity of 1.05E-6 Ω·m | |
Chemical properties
Property | Value |
---|---|
Carbon | 0.03 % Show Material materials with Carbon of 0.03 % |
Chromium | 10.5 - 12.5 % Show Material materials with Chromium of 10.5 - 12.5 % |
Manganese | 1 % Show Material materials with Manganese of 1 % |
Phosphorus | 0.04 % Show Material materials with Phosphorus of 0.04 % |
Silicon | 1 % Show Material materials with Silicon of 1 % |
Sulfur | 0.015 % Show Material materials with Sulfur of 0.015 % |
Titanium | 0.65 % Show Material materials with Titanium of 0.65 % |