General
Property | Temperature | Value |
---|---|---|
Density | 20.0 °C | 7.81 g/cm³ Show Material materials with Density of 7.81 g/cm³ |
Mechanical
Property | Temperature | Value |
---|---|---|
Elastic modulus | -100.0 °C | 217 GPa Show Material materials with Elastic modulus of 217 GPa |
20.0 °C | 210.27 - 212 GPa Show Material materials with Elastic modulus of 210.27 - 212 GPa | |
100.0 °C | 205.17 - 207 GPa Show Material materials with Elastic modulus of 205.17 - 207 GPa | |
200.0 °C | 198.68 - 199 GPa Show Material materials with Elastic modulus of 198.68 - 199 GPa | |
300.0 °C | 191.11 - 192 GPa Show Material materials with Elastic modulus of 191.11 - 192 GPa | |
400.0 °C | 182.31 - 184 GPa Show Material materials with Elastic modulus of 182.31 - 184 GPa | |
500.0 °C | 171.64 - 175 GPa Show Material materials with Elastic modulus of 171.64 - 175 GPa | |
600.0 °C | 164 GPa Show Material materials with Elastic modulus of 164 GPa | |
Elongation | 20.0 °C | 11 - 14 % Show Material materials with Elongation of 11 - 14 % |
Poisson's ratio | 20.0 °C | 0.28 [-] Show Material materials with Poisson's ratio of 0.28 [-] |
100.0 °C | 0.29 [-] Show Material materials with Poisson's ratio of 0.29 [-] | |
200.0 °C | 0.3 [-] Show Material materials with Poisson's ratio of 0.3 [-] | |
300.0 °C | 0.3 [-] Show Material materials with Poisson's ratio of 0.3 [-] | |
400.0 °C | 0.3 [-] Show Material materials with Poisson's ratio of 0.3 [-] | |
500.0 °C | 0.31 [-] Show Material materials with Poisson's ratio of 0.31 [-] | |
Reduction of area | 20.0 °C | 45 - 55 % Show Material materials with Reduction of area of 45 - 55 % |
Shear modulus | 20.0 °C | 81.88 GPa Show Material materials with Shear modulus of 81.88 GPa |
100.0 °C | 79.57 GPa Show Material materials with Shear modulus of 79.57 GPa | |
200.0 °C | 76.63 GPa Show Material materials with Shear modulus of 76.63 GPa | |
300.0 °C | 73.54 GPa Show Material materials with Shear modulus of 73.54 GPa | |
400.0 °C | 69.99 GPa Show Material materials with Shear modulus of 69.99 GPa | |
500.0 °C | 65.66 GPa Show Material materials with Shear modulus of 65.66 GPa | |
Tensile strength | 20.0 °C | 800 - 1200 MPa Show Material materials with Tensile strength of 800 - 1200 MPa |
Yield strength | 20.0 °C | 550 - 800 MPa Show Material materials with Yield strength of 550 - 800 MPa |
Thermal
Property | Temperature | Value | Comment |
---|---|---|---|
Coefficient of thermal expansion | -100.0 °C | 1.05E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.05E-5 1/K | |
20.0 °C | 1.15E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.15E-5 1/K | ||
100.0 °C | 1.21E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.21E-5 1/K | ||
200.0 °C | 1.27E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.27E-5 1/K | ||
300.0 °C | 1.32E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.32E-5 1/K | ||
400.0 °C | 1.36E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.36E-5 1/K | ||
500.0 °C | 1.4E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.4E-5 1/K | ||
600.0 °C | 1.44E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.44E-5 1/K | ||
Max service temperature, long | -40 - 0 °C Show Material materials with Max service temperature, long of -40 - 0 °C | ||
Melting point | 1382 - 1529 °C Show Material materials with Melting point of 1382 - 1529 °C | Typical for Chromium Molybdenum Steel | |
Specific heat capacity | -100.0 °C | 423 J/(kg·K) Show Material materials with Specific heat capacity of 423 J/(kg·K) | |
20.0 °C | 461 J/(kg·K) Show Material materials with Specific heat capacity of 461 J/(kg·K) | ||
100.0 °C | 479 J/(kg·K) Show Material materials with Specific heat capacity of 479 J/(kg·K) | ||
200.0 °C | 499 J/(kg·K) Show Material materials with Specific heat capacity of 499 J/(kg·K) | ||
300.0 °C | 517 J/(kg·K) Show Material materials with Specific heat capacity of 517 J/(kg·K) | ||
400.0 °C | 536 J/(kg·K) Show Material materials with Specific heat capacity of 536 J/(kg·K) | ||
500.0 °C | 558 J/(kg·K) Show Material materials with Specific heat capacity of 558 J/(kg·K) | ||
600.0 °C | 587 J/(kg·K) Show Material materials with Specific heat capacity of 587 J/(kg·K) | ||
Thermal conductivity | 20.0 °C | 39.6 W/(m·K) Show Material materials with Thermal conductivity of 39.6 W/(m·K) | |
100.0 °C | 41.6 W/(m·K) Show Material materials with Thermal conductivity of 41.6 W/(m·K) | ||
200.0 °C | 41.8 W/(m·K) Show Material materials with Thermal conductivity of 41.8 W/(m·K) | ||
300.0 °C | 40.3 W/(m·K) Show Material materials with Thermal conductivity of 40.3 W/(m·K) | ||
400.0 °C | 38.2 W/(m·K) Show Material materials with Thermal conductivity of 38.2 W/(m·K) | ||
500.0 °C | 36 W/(m·K) Show Material materials with Thermal conductivity of 36 W/(m·K) | ||
600.0 °C | 33.6 W/(m·K) Show Material materials with Thermal conductivity of 33.6 W/(m·K) | ||
Thermal diffusivity | 20.0 °C | 11 mm²/s Show Material materials with Thermal diffusivity of 11 mm²/s | |
100.0 °C | 10.8 mm²/s Show Material materials with Thermal diffusivity of 10.8 mm²/s | ||
200.0 °C | 10.1 mm²/s Show Material materials with Thermal diffusivity of 10.1 mm²/s | ||
300.0 °C | 9.2 mm²/s Show Material materials with Thermal diffusivity of 9.2 mm²/s | ||
400.0 °C | 8.1 mm²/s Show Material materials with Thermal diffusivity of 8.1 mm²/s | ||
500.0 °C | 7 mm²/s Show Material materials with Thermal diffusivity of 7 mm²/s | ||
600.0 °C | 5.7 mm²/s Show Material materials with Thermal diffusivity of 5.7 mm²/s | ||
Electrical
Property | Temperature | Value |
---|---|---|
Electrical resistivity | 20.0 °C | 2.63E-7 Ω·m Show Material materials with Electrical resistivity of 2.63E-7 Ω·m |
100.0 °C | 3.08E-7 Ω·m Show Material materials with Electrical resistivity of 3.08E-7 Ω·m | |
200.0 °C | 3.78E-7 Ω·m Show Material materials with Electrical resistivity of 3.78E-7 Ω·m | |
300.0 °C | 4.66E-7 Ω·m Show Material materials with Electrical resistivity of 4.66E-7 Ω·m | |
400.0 °C | 5.69E-7 Ω·m Show Material materials with Electrical resistivity of 5.69E-7 Ω·m | |
500.0 °C | 6.87E-7 Ω·m Show Material materials with Electrical resistivity of 6.87E-7 Ω·m | |
600.0 °C | 8.26E-7 Ω·m Show Material materials with Electrical resistivity of 8.26E-7 Ω·m | |
Chemical properties
Property | Value |
---|---|
Carbon | 0.3 - 0.37 % Show Material materials with Carbon of 0.3 - 0.37 % |
Chromium | 0.9 - 1.2 % Show Material materials with Chromium of 0.9 - 1.2 % |
Manganese | 0.6 - 0.9 % Show Material materials with Manganese of 0.6 - 0.9 % |
Molybdenum | 0.15 - 0.3 % Show Material materials with Molybdenum of 0.15 - 0.3 % |
Phosphorus | 0.04 % Show Material materials with Phosphorus of 0.04 % |
Silicon | 0.4 % Show Material materials with Silicon of 0.4 % |
Sulfur | 0.03 % Show Material materials with Sulfur of 0.03 % |
Do you have a technical question or need more information about this material?