General
Property | Temperature | Value |
---|---|---|
Density | 20.0 °C | 7.8 - 7.85 g/cm³ Show Material materials with Density of 7.8 - 7.85 g/cm³ |
Mechanical
Property | Temperature | Value |
---|---|---|
Elastic modulus | -100.0 °C | 217 GPa Show Material materials with Elastic modulus of 217 GPa |
20.0 °C | 208.26 - 212 GPa Show Material materials with Elastic modulus of 208.26 - 212 GPa | |
100.0 °C | 203.78 - 207 GPa Show Material materials with Elastic modulus of 203.78 - 207 GPa | |
200.0 °C | 195 - 199 GPa Show Material materials with Elastic modulus of 195 - 199 GPa | |
300.0 °C | 185 - 192 GPa Show Material materials with Elastic modulus of 185 - 192 GPa | |
400.0 °C | 175 - 184 GPa Show Material materials with Elastic modulus of 175 - 184 GPa | |
500.0 °C | 173.04 - 175 GPa Show Material materials with Elastic modulus of 173.04 - 175 GPa | |
600.0 °C | 164 GPa Show Material materials with Elastic modulus of 164 GPa | |
Elongation | 20.0 °C | 13 - 14 % Show Material materials with Elongation of 13 - 14 % |
Elongation, transverse | 20.0 °C | 11 - 12 % Show Material materials with Elongation, transverse of 11 - 12 % |
Poisson's ratio | 20.0 °C | 0.27 [-] Show Material materials with Poisson's ratio of 0.27 [-] |
100.0 °C | 0.27 [-] Show Material materials with Poisson's ratio of 0.27 [-] | |
200.0 °C | 0.28 [-] Show Material materials with Poisson's ratio of 0.28 [-] | |
300.0 °C | 0.28 [-] Show Material materials with Poisson's ratio of 0.28 [-] | |
400.0 °C | 0.28 [-] Show Material materials with Poisson's ratio of 0.28 [-] | |
500.0 °C | 0.28 [-] Show Material materials with Poisson's ratio of 0.28 [-] | |
Shear modulus | 20.0 °C | 81 - 82.04 GPa Show Material materials with Shear modulus of 81 - 82.04 GPa |
100.0 °C | 80.18 GPa Show Material materials with Shear modulus of 80.18 GPa | |
200.0 °C | 77.56 GPa Show Material materials with Shear modulus of 77.56 GPa | |
300.0 °C | 74.62 GPa Show Material materials with Shear modulus of 74.62 GPa | |
400.0 °C | 71.22 GPa Show Material materials with Shear modulus of 71.22 GPa | |
500.0 °C | 67.36 GPa Show Material materials with Shear modulus of 67.36 GPa | |
Tensile strength | 20.0 °C | 670 - 900 MPa Show Material materials with Tensile strength of 670 - 900 MPa |
Tensile strength, transverse | 20.0 °C | 670 - 900 MPa Show Material materials with Tensile strength, transverse of 670 - 900 MPa |
Yield strength | 20.0 °C | 360 - 390 MPa Show Material materials with Yield strength of 360 - 390 MPa |
Yield strength, transverse | 20.0 °C | 360 - 390 MPa Show Material materials with Yield strength, transverse of 360 - 390 MPa |
Thermal
Property | Temperature | Value | Comment |
---|---|---|---|
Coefficient of thermal expansion | -100.0 °C | 1.08E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.08E-5 1/K | |
20.0 °C | 1.19E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.19E-5 1/K | ||
100.0 °C | 1.11E-5 - 1.25E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.11E-5 - 1.25E-5 1/K | ||
200.0 °C | 1.21E-5 - 1.3E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.21E-5 - 1.3E-5 1/K | ||
300.0 °C | 1.29E-5 - 1.36E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.29E-5 - 1.36E-5 1/K | ||
400.0 °C | 1.35E-5 - 1.41E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.35E-5 - 1.41E-5 1/K | ||
500.0 °C | 1.45E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.45E-5 1/K | ||
600.0 °C | 1.49E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.49E-5 1/K | ||
Max service temperature | 500 °C Show Material materials with Max service temperature of 500 °C | Typical for Carbon Steel | |
Melting point | 1289 - 1478 °C Show Material materials with Melting point of 1289 - 1478 °C | Typical for High Carbon Steel | |
Specific heat capacity | -100.0 °C | 423 J/(kg·K) Show Material materials with Specific heat capacity of 423 J/(kg·K) | |
20.0 °C | 461 J/(kg·K) Show Material materials with Specific heat capacity of 461 J/(kg·K) | ||
100.0 °C | 479 J/(kg·K) Show Material materials with Specific heat capacity of 479 J/(kg·K) | ||
200.0 °C | 499 J/(kg·K) Show Material materials with Specific heat capacity of 499 J/(kg·K) | ||
300.0 °C | 517 J/(kg·K) Show Material materials with Specific heat capacity of 517 J/(kg·K) | ||
400.0 °C | 536 J/(kg·K) Show Material materials with Specific heat capacity of 536 J/(kg·K) | ||
500.0 °C | 558 J/(kg·K) Show Material materials with Specific heat capacity of 558 J/(kg·K) | ||
600.0 °C | 587 J/(kg·K) Show Material materials with Specific heat capacity of 587 J/(kg·K) | ||
Thermal conductivity | 20.0 °C | 41.7 - 51 W/(m·K) Show Material materials with Thermal conductivity of 41.7 - 51 W/(m·K) | |
100.0 °C | 43.4 - 49.9 W/(m·K) Show Material materials with Thermal conductivity of 43.4 - 49.9 W/(m·K) | ||
200.0 °C | 43.2 - 47.8 W/(m·K) Show Material materials with Thermal conductivity of 43.2 - 47.8 W/(m·K) | ||
300.0 °C | 41.4 - 44.8 W/(m·K) Show Material materials with Thermal conductivity of 41.4 - 44.8 W/(m·K) | ||
400.0 °C | 39.1 W/(m·K) Show Material materials with Thermal conductivity of 39.1 W/(m·K) | ||
500.0 °C | 36.7 W/(m·K) Show Material materials with Thermal conductivity of 36.7 W/(m·K) | ||
600.0 °C | 34.1 W/(m·K) Show Material materials with Thermal conductivity of 34.1 W/(m·K) | ||
Thermal diffusivity | 20.0 °C | 11.6 mm²/s Show Material materials with Thermal diffusivity of 11.6 mm²/s | |
100.0 °C | 11.3 mm²/s Show Material materials with Thermal diffusivity of 11.3 mm²/s | ||
200.0 °C | 10.5 mm²/s Show Material materials with Thermal diffusivity of 10.5 mm²/s | ||
300.0 °C | 9.5 mm²/s Show Material materials with Thermal diffusivity of 9.5 mm²/s | ||
400.0 °C | 8.3 mm²/s Show Material materials with Thermal diffusivity of 8.3 mm²/s | ||
500.0 °C | 7.1 mm²/s Show Material materials with Thermal diffusivity of 7.1 mm²/s | ||
600.0 °C | 5.8 mm²/s Show Material materials with Thermal diffusivity of 5.8 mm²/s | ||
Electrical
Property | Temperature | Value |
---|---|---|
Electrical resistivity | 20.0 °C | 1.3E-7 - 2.5E-7 Ω·m Show Material materials with Electrical resistivity of 1.3E-7 - 2.5E-7 Ω·m |
100.0 °C | 2.95E-7 Ω·m Show Material materials with Electrical resistivity of 2.95E-7 Ω·m | |
200.0 °C | 3.65E-7 Ω·m Show Material materials with Electrical resistivity of 3.65E-7 Ω·m | |
300.0 °C | 4.53E-7 Ω·m Show Material materials with Electrical resistivity of 4.53E-7 Ω·m | |
400.0 °C | 5.56E-7 Ω·m Show Material materials with Electrical resistivity of 5.56E-7 Ω·m | |
500.0 °C | 6.74E-7 Ω·m Show Material materials with Electrical resistivity of 6.74E-7 Ω·m | |
600.0 °C | 8.13E-7 Ω·m Show Material materials with Electrical resistivity of 8.13E-7 Ω·m | |
Chemical properties
Property | Value |
---|---|
Carbon | 0.57 - 0.65 % Show Material materials with Carbon of 0.57 - 0.65 % |
Manganese | 0.6 - 0.9 % Show Material materials with Manganese of 0.6 - 0.9 % |
Phosphorus | 0.05 % Show Material materials with Phosphorus of 0.05 % |
Silicon | 0.4 % Show Material materials with Silicon of 0.4 % |
Sulfur | 0.045 % Show Material materials with Sulfur of 0.045 % |