General
Property | Temperature | Value |
---|---|---|
Density | 20.0 °C | 7.85 g/cm³ Show Material materials with Density of 7.85 g/cm³ |
50.0 °C | 7.84 g/cm³ Show Material materials with Density of 7.84 g/cm³ | |
100.0 °C | 7.82 g/cm³ Show Material materials with Density of 7.82 g/cm³ | |
150.0 °C | 7.81 g/cm³ Show Material materials with Density of 7.81 g/cm³ | |
200.0 °C | 7.79 g/cm³ Show Material materials with Density of 7.79 g/cm³ | |
250.0 °C | 7.77 g/cm³ Show Material materials with Density of 7.77 g/cm³ | |
300.0 °C | 7.76 g/cm³ Show Material materials with Density of 7.76 g/cm³ | |
350.0 °C | 7.74 g/cm³ Show Material materials with Density of 7.74 g/cm³ | |
400.0 °C | 7.72 g/cm³ Show Material materials with Density of 7.72 g/cm³ | |
450.0 °C | 7.7 g/cm³ Show Material materials with Density of 7.7 g/cm³ | |
500.0 °C | 7.68 g/cm³ Show Material materials with Density of 7.68 g/cm³ | |
550.0 °C | 7.66 g/cm³ Show Material materials with Density of 7.66 g/cm³ | |
600.0 °C | 7.64 g/cm³ Show Material materials with Density of 7.64 g/cm³ | |
Mechanical
Property | Temperature | Value |
---|---|---|
Elastic modulus | -100.0 °C | 217 GPa Show Material materials with Elastic modulus of 217 GPa |
20.0 °C | 212 - 212.48 GPa Show Material materials with Elastic modulus of 212 - 212.48 GPa | |
50.0 °C | 211.6 GPa Show Material materials with Elastic modulus of 211.6 GPa | |
100.0 °C | 207 - 209 GPa Show Material materials with Elastic modulus of 207 - 209 GPa | |
150.0 °C | 205.52 GPa Show Material materials with Elastic modulus of 205.52 GPa | |
200.0 °C | 199 - 202 GPa Show Material materials with Elastic modulus of 199 - 202 GPa | |
250.0 °C | 197.67 GPa Show Material materials with Elastic modulus of 197.67 GPa | |
300.0 °C | 192 - 193.45 GPa Show Material materials with Elastic modulus of 192 - 193.45 GPa | |
350.0 °C | 189.23 GPa Show Material materials with Elastic modulus of 189.23 GPa | |
400.0 °C | 184 - 185 GPa Show Material materials with Elastic modulus of 184 - 185 GPa | |
450.0 °C | 180.41 GPa Show Material materials with Elastic modulus of 180.41 GPa | |
500.0 °C | 175 - 176 GPa Show Material materials with Elastic modulus of 175 - 176 GPa | |
550.0 °C | 171.28 GPa Show Material materials with Elastic modulus of 171.28 GPa | |
600.0 °C | 164 - 166.57 GPa Show Material materials with Elastic modulus of 164 - 166.57 GPa | |
Elongation | 20.0 °C | 18 - 20 % Show Material materials with Elongation of 18 - 20 % |
Poisson's ratio | 20.0 °C | 0.28 [-] Show Material materials with Poisson's ratio of 0.28 [-] |
50.0 °C | 0.28 [-] Show Material materials with Poisson's ratio of 0.28 [-] | |
100.0 °C | 0.28 [-] Show Material materials with Poisson's ratio of 0.28 [-] | |
150.0 °C | 0.29 [-] Show Material materials with Poisson's ratio of 0.29 [-] | |
200.0 °C | 0.29 [-] Show Material materials with Poisson's ratio of 0.29 [-] | |
250.0 °C | 0.29 [-] Show Material materials with Poisson's ratio of 0.29 [-] | |
300.0 °C | 0.29 [-] Show Material materials with Poisson's ratio of 0.29 [-] | |
350.0 °C | 0.3 [-] Show Material materials with Poisson's ratio of 0.3 [-] | |
400.0 °C | 0.3 [-] Show Material materials with Poisson's ratio of 0.3 [-] | |
450.0 °C | 0.3 [-] Show Material materials with Poisson's ratio of 0.3 [-] | |
500.0 °C | 0.3 [-] Show Material materials with Poisson's ratio of 0.3 [-] | |
550.0 °C | 0.31 [-] Show Material materials with Poisson's ratio of 0.31 [-] | |
600.0 °C | 0.31 [-] Show Material materials with Poisson's ratio of 0.31 [-] | |
Shear modulus | 20.0 °C | 82.8 GPa Show Material materials with Shear modulus of 82.8 GPa |
50.0 °C | 82.4 GPa Show Material materials with Shear modulus of 82.4 GPa | |
100.0 °C | 81.42 GPa Show Material materials with Shear modulus of 81.42 GPa | |
150.0 °C | 79.95 GPa Show Material materials with Shear modulus of 79.95 GPa | |
200.0 °C | 78.38 GPa Show Material materials with Shear modulus of 78.38 GPa | |
250.0 °C | 76.62 GPa Show Material materials with Shear modulus of 76.62 GPa | |
300.0 °C | 74.85 GPa Show Material materials with Shear modulus of 74.85 GPa | |
350.0 °C | 73.08 GPa Show Material materials with Shear modulus of 73.08 GPa | |
400.0 °C | 71.32 GPa Show Material materials with Shear modulus of 71.32 GPa | |
450.0 °C | 69.45 GPa Show Material materials with Shear modulus of 69.45 GPa | |
500.0 °C | 67.59 GPa Show Material materials with Shear modulus of 67.59 GPa | |
550.0 °C | 65.63 GPa Show Material materials with Shear modulus of 65.63 GPa | |
600.0 °C | 63.57 GPa Show Material materials with Shear modulus of 63.57 GPa | |
Tensile strength | 20.0 °C | 420 - 600 MPa Show Material materials with Tensile strength of 420 - 600 MPa |
200.0 °C | 390 MPa Show Material materials with Tensile strength of 390 MPa | |
250.0 °C | 390 MPa Show Material materials with Tensile strength of 390 MPa | |
300.0 °C | 390 MPa Show Material materials with Tensile strength of 390 MPa | |
350.0 °C | 390 MPa Show Material materials with Tensile strength of 390 MPa | |
400.0 °C | 385 MPa Show Material materials with Tensile strength of 385 MPa | |
450.0 °C | 365 MPa Show Material materials with Tensile strength of 365 MPa | |
500.0 °C | 335 MPa Show Material materials with Tensile strength of 335 MPa | |
Yield strength Rp0.2 | 20.0 °C | 240 - 300 MPa Show Material materials with Yield strength Rp0.2 of 240 - 300 MPa |
100.0 °C | 220 - 260 MPa Show Material materials with Yield strength Rp0.2 of 220 - 260 MPa | |
150.0 °C | 210 - 245 MPa Show Material materials with Yield strength Rp0.2 of 210 - 245 MPa | |
200.0 °C | 200 - 255 MPa Show Material materials with Yield strength Rp0.2 of 200 - 255 MPa | |
250.0 °C | 190 - 245 MPa Show Material materials with Yield strength Rp0.2 of 190 - 245 MPa | |
300.0 °C | 175 - 230 MPa Show Material materials with Yield strength Rp0.2 of 175 - 230 MPa | |
350.0 °C | 165 - 215 MPa Show Material materials with Yield strength Rp0.2 of 165 - 215 MPa | |
400.0 °C | 160 - 205 MPa Show Material materials with Yield strength Rp0.2 of 160 - 205 MPa | |
450.0 °C | 150 - 195 MPa Show Material materials with Yield strength Rp0.2 of 150 - 195 MPa | |
500.0 °C | 145 - 190 MPa Show Material materials with Yield strength Rp0.2 of 145 - 190 MPa | |
Thermal
Property | Temperature | Value | Comment |
---|---|---|---|
Coefficient of thermal expansion | -100.0 °C | 1.05E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.05E-5 1/K | |
20.0 °C | 1.15E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.15E-5 1/K | ||
100.0 °C | 1.21E-5 - 1.22E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.21E-5 - 1.22E-5 1/K | ||
200.0 °C | 1.27E-5 - 1.29E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.27E-5 - 1.29E-5 1/K | ||
300.0 °C | 1.32E-5 - 1.34E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.32E-5 - 1.34E-5 1/K | ||
400.0 °C | 1.36E-5 - 1.4E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.36E-5 - 1.4E-5 1/K | ||
500.0 °C | 1.4E-5 - 1.43E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.4E-5 - 1.43E-5 1/K | ||
600.0 °C | 1.44E-5 - 1.46E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.44E-5 - 1.46E-5 1/K | ||
Max service temperature, long | 0 - 530 °C Show Material materials with Max service temperature, long of 0 - 530 °C | ||
Melting point | 1382 - 1529 °C Show Material materials with Melting point of 1382 - 1529 °C | Typical for Chromium Molybdenum Steel | |
Specific heat capacity | -100.0 °C | 423 J/(kg·K) Show Material materials with Specific heat capacity of 423 J/(kg·K) | |
20.0 °C | 461 J/(kg·K) Show Material materials with Specific heat capacity of 461 J/(kg·K) | ||
100.0 °C | 479 - 500 J/(kg·K) Show Material materials with Specific heat capacity of 479 - 500 J/(kg·K) | ||
200.0 °C | 499 - 540 J/(kg·K) Show Material materials with Specific heat capacity of 499 - 540 J/(kg·K) | ||
300.0 °C | 517 - 580 J/(kg·K) Show Material materials with Specific heat capacity of 517 - 580 J/(kg·K) | ||
400.0 °C | 536 - 620 J/(kg·K) Show Material materials with Specific heat capacity of 536 - 620 J/(kg·K) | ||
500.0 °C | 558 - 690 J/(kg·K) Show Material materials with Specific heat capacity of 558 - 690 J/(kg·K) | ||
600.0 °C | 587 - 780 J/(kg·K) Show Material materials with Specific heat capacity of 587 - 780 J/(kg·K) | ||
Thermal conductivity | 20.0 °C | 45.9 W/(m·K) Show Material materials with Thermal conductivity of 45.9 W/(m·K) | |
100.0 °C | 46 - 46.4 W/(m·K) Show Material materials with Thermal conductivity of 46 - 46.4 W/(m·K) | ||
200.0 °C | 45.6 - 46 W/(m·K) Show Material materials with Thermal conductivity of 45.6 - 46 W/(m·K) | ||
300.0 °C | 43 - 43.5 W/(m·K) Show Material materials with Thermal conductivity of 43 - 43.5 W/(m·K) | ||
400.0 °C | 40.9 - 41 W/(m·K) Show Material materials with Thermal conductivity of 40.9 - 41 W/(m·K) | ||
500.0 °C | 38 - 38.2 W/(m·K) Show Material materials with Thermal conductivity of 38 - 38.2 W/(m·K) | ||
600.0 °C | 35.5 - 36 W/(m·K) Show Material materials with Thermal conductivity of 35.5 - 36 W/(m·K) | ||
Thermal diffusivity | 20.0 °C | 12.7 mm²/s Show Material materials with Thermal diffusivity of 12.7 mm²/s | |
100.0 °C | 12 mm²/s Show Material materials with Thermal diffusivity of 12 mm²/s | ||
200.0 °C | 11 mm²/s Show Material materials with Thermal diffusivity of 11 mm²/s | ||
300.0 °C | 9.9 mm²/s Show Material materials with Thermal diffusivity of 9.9 mm²/s | ||
400.0 °C | 8.7 mm²/s Show Material materials with Thermal diffusivity of 8.7 mm²/s | ||
500.0 °C | 7.3 mm²/s Show Material materials with Thermal diffusivity of 7.3 mm²/s | ||
600.0 °C | 6 mm²/s Show Material materials with Thermal diffusivity of 6 mm²/s | ||
Electrical
Property | Temperature | Value |
---|---|---|
Electrical resistivity | 20.0 °C | 2.27E-7 - 2.37E-7 Ω·m Show Material materials with Electrical resistivity of 2.27E-7 - 2.37E-7 Ω·m |
50.0 °C | 2.56E-7 Ω·m Show Material materials with Electrical resistivity of 2.56E-7 Ω·m | |
100.0 °C | 2.76E-7 - 2.88E-7 Ω·m Show Material materials with Electrical resistivity of 2.76E-7 - 2.88E-7 Ω·m | |
150.0 °C | 3.21E-7 Ω·m Show Material materials with Electrical resistivity of 3.21E-7 Ω·m | |
200.0 °C | 3.46E-7 - 3.59E-7 Ω·m Show Material materials with Electrical resistivity of 3.46E-7 - 3.59E-7 Ω·m | |
250.0 °C | 4.01E-7 Ω·m Show Material materials with Electrical resistivity of 4.01E-7 Ω·m | |
300.0 °C | 4.3E-7 - 4.45E-7 Ω·m Show Material materials with Electrical resistivity of 4.3E-7 - 4.45E-7 Ω·m | |
350.0 °C | 4.95E-7 Ω·m Show Material materials with Electrical resistivity of 4.95E-7 Ω·m | |
400.0 °C | 5.3E-7 - 5.48E-7 Ω·m Show Material materials with Electrical resistivity of 5.3E-7 - 5.48E-7 Ω·m | |
450.0 °C | 6.06E-7 Ω·m Show Material materials with Electrical resistivity of 6.06E-7 Ω·m | |
500.0 °C | 6.48E-7 - 6.63E-7 Ω·m Show Material materials with Electrical resistivity of 6.48E-7 - 6.63E-7 Ω·m | |
550.0 °C | 7.28E-7 Ω·m Show Material materials with Electrical resistivity of 7.28E-7 Ω·m | |
600.0 °C | 7.8E-7 - 7.97E-7 Ω·m Show Material materials with Electrical resistivity of 7.8E-7 - 7.97E-7 Ω·m | |
Chemical properties
Property | Value |
---|---|
Carbon | 0.08 - 0.18 % Show Material materials with Carbon of 0.08 - 0.18 % |
Chromium | 0.7 - 1.15 % Show Material materials with Chromium of 0.7 - 1.15 % |
Manganese | 0.4 - 1 % Show Material materials with Manganese of 0.4 - 1 % |
Molybdenum | 0.4 - 0.8 % Show Material materials with Molybdenum of 0.4 - 0.8 % |
Phosphorus | 0.04 % Show Material materials with Phosphorus of 0.04 % |
Silicon | 0.1 - 0.4 % Show Material materials with Silicon of 0.1 - 0.4 % |
Sulfur | 0.03 % Show Material materials with Sulfur of 0.03 % |
Do you have a technical question or need more information about this material?
Post it as a comment below and receive answers from engineers and other community members.