General
Property | Temperature | Value |
---|---|---|
Density | 20.0 °C | 7.96 g/cm³ Show Material materials with Density of 7.96 g/cm³ |
Mechanical
Property | Temperature | Value | Comment |
---|---|---|---|
Elastic modulus | -100.0 °C | 206 GPa Show Material materials with Elastic modulus of 206 GPa | |
20.0 °C | 196 GPa Show Material materials with Elastic modulus of 196 GPa | ||
100.0 °C | 190 GPa Show Material materials with Elastic modulus of 190 GPa | ||
200.0 °C | 182 GPa Show Material materials with Elastic modulus of 182 GPa | ||
300.0 °C | 174 GPa Show Material materials with Elastic modulus of 174 GPa | ||
400.0 °C | 166 GPa Show Material materials with Elastic modulus of 166 GPa | ||
500.0 °C | 158 GPa Show Material materials with Elastic modulus of 158 GPa | ||
600.0 °C | 150 GPa Show Material materials with Elastic modulus of 150 GPa | ||
700.0 °C | 142 GPa Show Material materials with Elastic modulus of 142 GPa | ||
800.0 °C | 134 GPa Show Material materials with Elastic modulus of 134 GPa | ||
900.0 °C | 127 GPa Show Material materials with Elastic modulus of 127 GPa | ||
1000.0 °C | 120 GPa Show Material materials with Elastic modulus of 120 GPa | ||
Elongation | 20.0 °C | 40 % Show Material materials with Elongation of 40 % | |
Elongation, transverse | 20.0 °C | 30 % Show Material materials with Elongation, transverse of 30 % | |
Poisson's ratio | 23.0 °C | 0.3 [-] Show Material materials with Poisson's ratio of 0.3 [-] | Typical for Austenitic Stainless Steel |
Shear modulus | 23.0 °C | 77 GPa Show Material materials with Shear modulus of 77 GPa | Typical for Austenitic Stainless Steel |
Tensile strength | 20.0 °C | 490 - 690 MPa Show Material materials with Tensile strength of 490 - 690 MPa | |
Tensile strength, transverse | 20.0 °C | 490 - 690 MPa Show Material materials with Tensile strength, transverse of 490 - 690 MPa | |
Yield strength | 20.0 °C | 190 MPa Show Material materials with Yield strength of 190 MPa | |
Yield strength Rp0.2 | 50.0 °C | 182 MPa Show Material materials with Yield strength Rp0.2 of 182 MPa | |
100.0 °C | 166 MPa Show Material materials with Yield strength Rp0.2 of 166 MPa | ||
150.0 °C | 152 MPa Show Material materials with Yield strength Rp0.2 of 152 MPa | ||
200.0 °C | 137 MPa Show Material materials with Yield strength Rp0.2 of 137 MPa | ||
250.0 °C | 127 MPa Show Material materials with Yield strength Rp0.2 of 127 MPa | ||
300.0 °C | 118 MPa Show Material materials with Yield strength Rp0.2 of 118 MPa | ||
350.0 °C | 113 MPa Show Material materials with Yield strength Rp0.2 of 113 MPa | ||
400.0 °C | 108 MPa Show Material materials with Yield strength Rp0.2 of 108 MPa | ||
450.0 °C | 103 MPa Show Material materials with Yield strength Rp0.2 of 103 MPa | ||
500.0 °C | 100 MPa Show Material materials with Yield strength Rp0.2 of 100 MPa | ||
550.0 °C | 98 MPa Show Material materials with Yield strength Rp0.2 of 98 MPa | ||
Yield strength Rp1.0 | 20.0 °C | 225 MPa Show Material materials with Yield strength Rp1.0 of 225 MPa | |
50.0 °C | 217 MPa Show Material materials with Yield strength Rp1.0 of 217 MPa | ||
100.0 °C | 199 MPa Show Material materials with Yield strength Rp1.0 of 199 MPa | ||
150.0 °C | 181 MPa Show Material materials with Yield strength Rp1.0 of 181 MPa | ||
200.0 °C | 167 MPa Show Material materials with Yield strength Rp1.0 of 167 MPa | ||
250.0 °C | 157 MPa Show Material materials with Yield strength Rp1.0 of 157 MPa | ||
300.0 °C | 145 MPa Show Material materials with Yield strength Rp1.0 of 145 MPa | ||
350.0 °C | 139 MPa Show Material materials with Yield strength Rp1.0 of 139 MPa | ||
400.0 °C | 135 MPa Show Material materials with Yield strength Rp1.0 of 135 MPa | ||
450.0 °C | 130 MPa Show Material materials with Yield strength Rp1.0 of 130 MPa | ||
500.0 °C | 128 MPa Show Material materials with Yield strength Rp1.0 of 128 MPa | ||
550.0 °C | 127 MPa Show Material materials with Yield strength Rp1.0 of 127 MPa | ||
Yield strength Rp1.0, transverse | 20.0 °C | 225 MPa Show Material materials with Yield strength Rp1.0, transverse of 225 MPa | |
Yield strength, transverse | 20.0 °C | 190 MPa Show Material materials with Yield strength, transverse of 190 MPa |
Thermal
Property | Temperature | Value | Comment |
---|---|---|---|
Coefficient of thermal expansion | -100.0 °C | 1.49E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.49E-5 1/K | |
20.0 °C | 1.61E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.61E-5 1/K | ||
100.0 °C | 1.67E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.67E-5 1/K | ||
200.0 °C | 1.72E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.72E-5 1/K | ||
300.0 °C | 1.77E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.77E-5 1/K | ||
400.0 °C | 1.81E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.81E-5 1/K | ||
500.0 °C | 1.84E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.84E-5 1/K | ||
600.0 °C | 1.88E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.88E-5 1/K | ||
700.0 °C | 1.91E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.91E-5 1/K | ||
800.0 °C | 1.94E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.94E-5 1/K | ||
900.0 °C | 1.97E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.97E-5 1/K | ||
1000.0 °C | 2E-5 1/K Show Material materials with Coefficient of thermal expansion of 2E-5 1/K | ||
Melting point | 1230 - 1480 °C Show Material materials with Melting point of 1230 - 1480 °C | Typical for Austenitic Stainless Steel | |
Specific heat capacity | -100.0 °C | 440 J/(kg·K) Show Material materials with Specific heat capacity of 440 J/(kg·K) | |
20.0 °C | 472 J/(kg·K) Show Material materials with Specific heat capacity of 472 J/(kg·K) | ||
100.0 °C | 487 J/(kg·K) Show Material materials with Specific heat capacity of 487 J/(kg·K) | ||
200.0 °C | 503 J/(kg·K) Show Material materials with Specific heat capacity of 503 J/(kg·K) | ||
300.0 °C | 512 J/(kg·K) Show Material materials with Specific heat capacity of 512 J/(kg·K) | ||
400.0 °C | 520 J/(kg·K) Show Material materials with Specific heat capacity of 520 J/(kg·K) | ||
500.0 °C | 530 J/(kg·K) Show Material materials with Specific heat capacity of 530 J/(kg·K) | ||
600.0 °C | 541 J/(kg·K) Show Material materials with Specific heat capacity of 541 J/(kg·K) | ||
700.0 °C | 551 J/(kg·K) Show Material materials with Specific heat capacity of 551 J/(kg·K) | ||
800.0 °C | 559 J/(kg·K) Show Material materials with Specific heat capacity of 559 J/(kg·K) | ||
900.0 °C | 565 J/(kg·K) Show Material materials with Specific heat capacity of 565 J/(kg·K) | ||
1000.0 °C | 571 J/(kg·K) Show Material materials with Specific heat capacity of 571 J/(kg·K) | ||
Thermal conductivity | 20.0 °C | 13.3 W/(m·K) Show Material materials with Thermal conductivity of 13.3 W/(m·K) | |
100.0 °C | 14.9 W/(m·K) Show Material materials with Thermal conductivity of 14.9 W/(m·K) | ||
200.0 °C | 16.5 W/(m·K) Show Material materials with Thermal conductivity of 16.5 W/(m·K) | ||
300.0 °C | 18.1 W/(m·K) Show Material materials with Thermal conductivity of 18.1 W/(m·K) | ||
400.0 °C | 19.5 W/(m·K) Show Material materials with Thermal conductivity of 19.5 W/(m·K) | ||
500.0 °C | 21 W/(m·K) Show Material materials with Thermal conductivity of 21 W/(m·K) | ||
600.0 °C | 22.4 W/(m·K) Show Material materials with Thermal conductivity of 22.4 W/(m·K) | ||
700.0 °C | 23.8 W/(m·K) Show Material materials with Thermal conductivity of 23.8 W/(m·K) | ||
800.0 °C | 25.2 W/(m·K) Show Material materials with Thermal conductivity of 25.2 W/(m·K) | ||
Thermal diffusivity | 20.0 °C | 3.5 mm²/s Show Material materials with Thermal diffusivity of 3.5 mm²/s | |
100.0 °C | 3.8 mm²/s Show Material materials with Thermal diffusivity of 3.8 mm²/s | ||
200.0 °C | 4 mm²/s Show Material materials with Thermal diffusivity of 4 mm²/s | ||
300.0 °C | 4.3 mm²/s Show Material materials with Thermal diffusivity of 4.3 mm²/s | ||
400.0 °C | 4.5 mm²/s Show Material materials with Thermal diffusivity of 4.5 mm²/s | ||
500.0 °C | 4.7 mm²/s Show Material materials with Thermal diffusivity of 4.7 mm²/s | ||
600.0 °C | 4.8 mm²/s Show Material materials with Thermal diffusivity of 4.8 mm²/s | ||
700.0 °C | 5.1 mm²/s Show Material materials with Thermal diffusivity of 5.1 mm²/s | ||
800.0 °C | 5.4 mm²/s Show Material materials with Thermal diffusivity of 5.4 mm²/s | ||
Electrical
Property | Temperature | Value |
---|---|---|
Electrical resistivity | 20.0 °C | 7.91E-7 Ω·m Show Material materials with Electrical resistivity of 7.91E-7 Ω·m |
100.0 °C | 8.45E-7 Ω·m Show Material materials with Electrical resistivity of 8.45E-7 Ω·m | |
200.0 °C | 9.19E-7 Ω·m Show Material materials with Electrical resistivity of 9.19E-7 Ω·m | |
300.0 °C | 9.77E-7 Ω·m Show Material materials with Electrical resistivity of 9.77E-7 Ω·m | |
400.0 °C | 1.03E-6 Ω·m Show Material materials with Electrical resistivity of 1.03E-6 Ω·m | |
500.0 °C | 1.08E-6 Ω·m Show Material materials with Electrical resistivity of 1.08E-6 Ω·m | |
600.0 °C | 1.12E-6 Ω·m Show Material materials with Electrical resistivity of 1.12E-6 Ω·m | |
700.0 °C | 1.15E-6 Ω·m Show Material materials with Electrical resistivity of 1.15E-6 Ω·m | |
800.0 °C | 1.18E-6 Ω·m Show Material materials with Electrical resistivity of 1.18E-6 Ω·m | |
Chemical properties
Property | Value |
---|---|
Carbon | 0.03 % Show Material materials with Carbon of 0.03 % |
Chromium | 16.5 - 18.5 % Show Material materials with Chromium of 16.5 - 18.5 % |
Manganese | 2 % Show Material materials with Manganese of 2 % |
Molybdenum | 2 - 2.5 % Show Material materials with Molybdenum of 2 - 2.5 % |
Nickel | 10 - 13 % Show Material materials with Nickel of 10 - 13 % |
Nitrogen | 0.11 % Show Material materials with Nitrogen of 0.11 % |
Phosphorus | 0.05 % Show Material materials with Phosphorus of 0.05 % |
Silicon | 1 % Show Material materials with Silicon of 1 % |
Sulfur | 0.015 % Show Material materials with Sulfur of 0.015 % |
Do you have a technical question or need more information about this material?