EN 10028-7 Grade X2CrNiN23-4 solution annealed (+AT)

Want to keep this datasheet? Save it now in your required format

Description

The austenitic-ferritic steel X2CrNiN23-4 is a stainless duplex steel of high strength and hardness, favorable resistance to general corrosion, pitting corrosion and especially to stress corrosion. Furthermore resistance to intercrystalline corrosion also in the sensitized resp. welded condition. The sort is acc. to DIN EN 10095 applicable as heat resistant steel. Application: for lightweight constructions of longer durability and higher reliability, in the apparatus construction for heat-exchanger and pipelines in chloride-containing media, hydraulic tubes, feeder water preheater, agitator shafts and steam heating systems

Related Standards

Equivalent Materials

This material data has been provided by WIAM.

All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

Ashby charts

See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Properties

General

PropertyTemperatureValue

Density

20.0 °C

7.8 g/cm³

Show Material materials with Density of 7.8 g/cm³

Mechanical

PropertyTemperatureValueComment

Elastic modulus

20.0 °C

200 - 212 GPa

Show Material materials with Elastic modulus of 200 - 212 GPa

100.0 °C

194 - 206 GPa

Show Material materials with Elastic modulus of 194 - 206 GPa

200.0 °C

186 GPa

Show Material materials with Elastic modulus of 186 GPa

300.0 °C

180 GPa

Show Material materials with Elastic modulus of 180 GPa

Elongation

20.0 °C

20 - 25 %

Show Material materials with Elongation of 20 - 25 %

Elongation A80

20.0 °C

20 - 25 %

Show Material materials with Elongation A80 of 20 - 25 %

Elongation A80, transverse

20.0 °C

20 - 25 %

Show Material materials with Elongation A80, transverse of 20 - 25 %

Elongation, transverse

20.0 °C

20 - 25 %

Show Material materials with Elongation, transverse of 20 - 25 %

Poisson's ratio

23.0 °C

0.3 [-]

Show Material materials with Poisson's ratio of 0.3 [-]

Typical for Duplex Stainless Steel

Shear modulus

23.0 °C

77 GPa

Show Material materials with Shear modulus of 77 GPa

Typical for Duplex Stainless Steel

Tensile strength

20.0 °C

600 - 850 MPa

Show Material materials with Tensile strength of 600 - 850 MPa

50.0 °C

577 MPa

Show Material materials with Tensile strength of 577 MPa

100.0 °C

540 MPa

Show Material materials with Tensile strength of 540 MPa

150.0 °C

520 MPa

Show Material materials with Tensile strength of 520 MPa

200.0 °C

500 MPa

Show Material materials with Tensile strength of 500 MPa

250.0 °C

490 MPa

Show Material materials with Tensile strength of 490 MPa

Unlock all property charts

Tensile strength, transverse

20.0 °C

600 - 850 MPa

Show Material materials with Tensile strength, transverse of 600 - 850 MPa

Yield strength Rp0.2

50.0 °C

374 MPa

Show Material materials with Yield strength Rp0.2 of 374 MPa

100.0 °C

330 MPa

Show Material materials with Yield strength Rp0.2 of 330 MPa

150.0 °C

300 MPa

Show Material materials with Yield strength Rp0.2 of 300 MPa

200.0 °C

280 MPa

Show Material materials with Yield strength Rp0.2 of 280 MPa

250.0 °C

265 MPa

Show Material materials with Yield strength Rp0.2 of 265 MPa

Unlock all property charts

Yield strength Rp0.2, transverse

20.0 °C

385 - 420 MPa

Show Material materials with Yield strength Rp0.2, transverse of 385 - 420 MPa

Thermal

PropertyTemperatureValueComment

Coefficient of thermal expansion

100.0 °C

1.3E-5 - 1.33E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.3E-5 - 1.33E-5 1/K

200.0 °C

1.35E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.35E-5 1/K

300.0 °C

1.4E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.4E-5 1/K

Unlock all property charts

Max service temperature

300 °C

Show Material materials with Max service temperature of 300 °C

Typical for Duplex Stainless Steel

Melting point

1375 - 1450 °C

Show Material materials with Melting point of 1375 - 1450 °C

Typical for Duplex Stainless Steel

Specific heat capacity

20.0 °C

500 J/(kg·K)

Show Material materials with Specific heat capacity of 500 J/(kg·K)

Thermal conductivity

20.0 °C

13.4 - 15 W/(m·K)

Show Material materials with Thermal conductivity of 13.4 - 15 W/(m·K)

100.0 °C

14.9 W/(m·K)

Show Material materials with Thermal conductivity of 14.9 W/(m·K)

Unlock all property charts

Electrical

PropertyTemperatureValue

Electrical resistivity

20.0 °C

7.85E-7 - 8E-7 Ω·m

Show Material materials with Electrical resistivity of 7.85E-7 - 8E-7 Ω·m

100.0 °C

8.44E-7 Ω·m

Show Material materials with Electrical resistivity of 8.44E-7 Ω·m

Unlock all property charts

Chemical properties

PropertyValue

Carbon

0.03 %

Show Material materials with Carbon of 0.03 %

Chromium

22 - 24 %

Show Material materials with Chromium of 22 - 24 %

Copper

0.1 - 0.6 %

Show Material materials with Copper of 0.1 - 0.6 %

Manganese

2 %

Show Material materials with Manganese of 2 %

Molybdenum

0.1 - 0.6 %

Show Material materials with Molybdenum of 0.1 - 0.6 %

Nickel

3.5 - 5.5 %

Show Material materials with Nickel of 3.5 - 5.5 %

Nitrogen

0.05 - 0.2 %

Show Material materials with Nitrogen of 0.05 - 0.2 %

Phosphorus

0.04 %

Show Material materials with Phosphorus of 0.04 %

Silicon

1 %

Show Material materials with Silicon of 1 %

Sulfur

0.015 %

Show Material materials with Sulfur of 0.015 %