DIN 17440 Grade X20Cr13 soft annealed (+A)

Want to keep this datasheet? Save it now in your required format

Description

Propertties: - good corrosion resistance to water and steam - is able for high gloss polishing - application temperature: -40 up to 550°C Application: - for construction elements, requiring higher strengths because higher mechanical loadings - axis, parts for pumps, plunger, valve cone, nozzle pin, propeller for ships - also for beater bars and surgical instruments

Related Standards

Equivalent Materials

This material data has been provided by WIAM.

All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

Ashby charts

See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Properties

General

PropertyTemperatureValue

Density

20.0 °C

7.7 - 7.71 g/cm³

Show Material materials with Density of 7.7 - 7.71 g/cm³

Mechanical

PropertyTemperatureValueComment

Elastic modulus

20.0 °C

216 - 222 GPa

Show Material materials with Elastic modulus of 216 - 222 GPa

100.0 °C

213 - 216 GPa

Show Material materials with Elastic modulus of 213 - 216 GPa

200.0 °C

207 - 209 GPa

Show Material materials with Elastic modulus of 207 - 209 GPa

300.0 °C

200 - 201 GPa

Show Material materials with Elastic modulus of 200 - 201 GPa

400.0 °C

192 GPa

Show Material materials with Elastic modulus of 192 GPa

500.0 °C

183 GPa

Show Material materials with Elastic modulus of 183 GPa

600.0 °C

174 GPa

Show Material materials with Elastic modulus of 174 GPa

Hardness, Brinell

20.0 °C

230 [-]

Show Material materials with Hardness, Brinell of 230 [-]

Hardness, Vickers

20.0 °C

230 [-]

Show Material materials with Hardness, Vickers of 230 [-]

Poisson's ratio

23.0 °C

0.3 [-]

Show Material materials with Poisson's ratio of 0.3 [-]

Typical for Martensitic Stainless Steel

Shear modulus

23.0 °C

77 GPa

Show Material materials with Shear modulus of 77 GPa

Typical for Martensitic Stainless Steel

Tensile strength

20.0 °C

740 MPa

Show Material materials with Tensile strength of 740 MPa

Thermal

PropertyTemperatureValueComment

Coefficient of thermal expansion

20.0 °C

1.02E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.02E-5 1/K

100.0 °C

1.05E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.05E-5 1/K

200.0 °C

1.09E-5 - 1.1E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.09E-5 - 1.1E-5 1/K

300.0 °C

1.13E-5 - 1.15E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.13E-5 - 1.15E-5 1/K

400.0 °C

1.16E-5 - 1.2E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.16E-5 - 1.2E-5 1/K

500.0 °C

1.2E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.2E-5 1/K

600.0 °C

1.22E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.22E-5 1/K

Unlock all property charts

Max service temperature, long

-40 - 550 °C

Show Material materials with Max service temperature, long of -40 - 550 °C

Melting point

1370 - 1530 °C

Show Material materials with Melting point of 1370 - 1530 °C

Typical for Martensitic Stainless Steel

Specific heat capacity

20.0 °C

439 - 460 J/(kg·K)

Show Material materials with Specific heat capacity of 439 - 460 J/(kg·K)

100.0 °C

474 J/(kg·K)

Show Material materials with Specific heat capacity of 474 J/(kg·K)

200.0 °C

498 J/(kg·K)

Show Material materials with Specific heat capacity of 498 J/(kg·K)

300.0 °C

517 J/(kg·K)

Show Material materials with Specific heat capacity of 517 J/(kg·K)

400.0 °C

538 J/(kg·K)

Show Material materials with Specific heat capacity of 538 J/(kg·K)

500.0 °C

564 J/(kg·K)

Show Material materials with Specific heat capacity of 564 J/(kg·K)

600.0 °C

598 J/(kg·K)

Show Material materials with Specific heat capacity of 598 J/(kg·K)

Unlock all property charts

Thermal conductivity

20.0 °C

24.6 - 30 W/(m·K)

Show Material materials with Thermal conductivity of 24.6 - 30 W/(m·K)

100.0 °C

24.7 W/(m·K)

Show Material materials with Thermal conductivity of 24.7 W/(m·K)

200.0 °C

25 W/(m·K)

Show Material materials with Thermal conductivity of 25 W/(m·K)

300.0 °C

25.2 W/(m·K)

Show Material materials with Thermal conductivity of 25.2 W/(m·K)

400.0 °C

25.5 W/(m·K)

Show Material materials with Thermal conductivity of 25.5 W/(m·K)

500.0 °C

25.8 W/(m·K)

Show Material materials with Thermal conductivity of 25.8 W/(m·K)

600.0 °C

26 W/(m·K)

Show Material materials with Thermal conductivity of 26 W/(m·K)

Unlock all property charts

Thermal diffusivity

20.0 °C

7.3 mm²/s

Show Material materials with Thermal diffusivity of 7.3 mm²/s

100.0 °C

6.4 mm²/s

Show Material materials with Thermal diffusivity of 6.4 mm²/s

200.0 °C

6.1 mm²/s

Show Material materials with Thermal diffusivity of 6.1 mm²/s

300.0 °C

5.8 mm²/s

Show Material materials with Thermal diffusivity of 5.8 mm²/s

400.0 °C

5.4 mm²/s

Show Material materials with Thermal diffusivity of 5.4 mm²/s

500.0 °C

4.8 mm²/s

Show Material materials with Thermal diffusivity of 4.8 mm²/s

600.0 °C

4.1 mm²/s

Show Material materials with Thermal diffusivity of 4.1 mm²/s

Unlock all property charts

Electrical

PropertyTemperatureValue

Electrical resistivity

20.0 °C

5.87E-7 - 6E-7 Ω·m

Show Material materials with Electrical resistivity of 5.87E-7 - 6E-7 Ω·m

100.0 °C

6.55E-7 Ω·m

Show Material materials with Electrical resistivity of 6.55E-7 Ω·m

200.0 °C

7.38E-7 Ω·m

Show Material materials with Electrical resistivity of 7.38E-7 Ω·m

300.0 °C

8.19E-7 Ω·m

Show Material materials with Electrical resistivity of 8.19E-7 Ω·m

400.0 °C

8.96E-7 Ω·m

Show Material materials with Electrical resistivity of 8.96E-7 Ω·m

500.0 °C

9.7E-7 Ω·m

Show Material materials with Electrical resistivity of 9.7E-7 Ω·m

600.0 °C

1.04E-6 Ω·m

Show Material materials with Electrical resistivity of 1.04E-6 Ω·m

Unlock all property charts

Chemical properties

PropertyValue

Carbon

0.16 - 0.25 %

Show Material materials with Carbon of 0.16 - 0.25 %

Chromium

12 - 14 %

Show Material materials with Chromium of 12 - 14 %

Manganese

1 - 1.5 %

Show Material materials with Manganese of 1 - 1.5 %

Phosphorus

0.04 - 0.05 %

Show Material materials with Phosphorus of 0.04 - 0.05 %

Silicon

1 %

Show Material materials with Silicon of 1 %

Sulfur

0.015 - 0.03 %

Show Material materials with Sulfur of 0.015 - 0.03 %