DIN 17440 Grade X2CrNiMo17-12-2 solution annealed (+AT)

Want to keep this datasheet? Save it now in your required format

Description

The material X2CrNiMo17-12-2, mat. no. 1.4404, is an modification of the X5CrNiMo17-12-2 (1.4401). It shows high corrosion resistance, also because of the lower C-content, to not oxidising acids and chloride containing media, is high polishable and very good cold formable. According DIN 17440 : 1996-09 the material is used for flat products and rods (for pressure vessels), forgings and wires, acc. DIN 17441 : 1997-02 for cold rolled sheet and slit strip for pressure vessels. With the lower C-content the steel has an higher resistance to intercrystalline corrosion, both in the delivery condition and in the welded condition. The limiting temperature (operating time up to 100000 h no intercrystalline corrosion) amounts to 400 degrees C. According to DIN 17440 : 1985-07 (X 2 CrNiMo 17 13 2) resp. DIN EN 10088-1,-2,-3 : 1995-08 applies: application in the chemical apparatus construction and the cellulose industry, textile industry, pharmaceutical industry and in sewage plants.

Related Standards

Equivalent Materials

This material data has been provided by WIAM.

All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

Ashby charts

See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Properties

General

PropertyTemperatureValue

Density

20.0 °C

7.96 - 7.98 g/cm³

Show Material materials with Density of 7.96 - 7.98 g/cm³

Mechanical

PropertyTemperatureValueComment

Elastic modulus

-100.0 °C

206 GPa

Show Material materials with Elastic modulus of 206 GPa

20.0 °C

196 - 200 GPa

Show Material materials with Elastic modulus of 196 - 200 GPa

100.0 °C

190 - 194 GPa

Show Material materials with Elastic modulus of 190 - 194 GPa

200.0 °C

182 - 186 GPa

Show Material materials with Elastic modulus of 182 - 186 GPa

300.0 °C

174 - 179 GPa

Show Material materials with Elastic modulus of 174 - 179 GPa

400.0 °C

166 - 172 GPa

Show Material materials with Elastic modulus of 166 - 172 GPa

500.0 °C

158 - 165 GPa

Show Material materials with Elastic modulus of 158 - 165 GPa

600.0 °C

150 GPa

Show Material materials with Elastic modulus of 150 GPa

700.0 °C

142 GPa

Show Material materials with Elastic modulus of 142 GPa

800.0 °C

134 GPa

Show Material materials with Elastic modulus of 134 GPa

900.0 °C

127 GPa

Show Material materials with Elastic modulus of 127 GPa

1000.0 °C

120 GPa

Show Material materials with Elastic modulus of 120 GPa

Elongation

20.0 °C

38 %

Show Material materials with Elongation of 38 %

Elongation A80

20.0 °C

35 %

Show Material materials with Elongation A80 of 35 %

Elongation A80, transverse

20.0 °C

40 %

Show Material materials with Elongation A80, transverse of 40 %

Elongation, transverse

20.0 °C

40 %

Show Material materials with Elongation, transverse of 40 %

Poisson's ratio

23.0 °C

0.3 [-]

Show Material materials with Poisson's ratio of 0.3 [-]

Typical for Austenitic Stainless Steel

Shear modulus

23.0 °C

77 GPa

Show Material materials with Shear modulus of 77 GPa

Typical for Austenitic Stainless Steel

Tensile strength

20.0 °C

530 - 680 MPa

Show Material materials with Tensile strength of 530 - 680 MPa

Tensile strength, transverse

20.0 °C

530 - 680 MPa

Show Material materials with Tensile strength, transverse of 530 - 680 MPa

Yield strength Rp0.2

20.0 °C

225 MPa

Show Material materials with Yield strength Rp0.2 of 225 MPa

100.0 °C

166 MPa

Show Material materials with Yield strength Rp0.2 of 166 MPa

150.0 °C

152 MPa

Show Material materials with Yield strength Rp0.2 of 152 MPa

200.0 °C

137 MPa

Show Material materials with Yield strength Rp0.2 of 137 MPa

250.0 °C

127 MPa

Show Material materials with Yield strength Rp0.2 of 127 MPa

300.0 °C

118 MPa

Show Material materials with Yield strength Rp0.2 of 118 MPa

350.0 °C

113 MPa

Show Material materials with Yield strength Rp0.2 of 113 MPa

400.0 °C

108 MPa

Show Material materials with Yield strength Rp0.2 of 108 MPa

450.0 °C

103 MPa

Show Material materials with Yield strength Rp0.2 of 103 MPa

500.0 °C

100 MPa

Show Material materials with Yield strength Rp0.2 of 100 MPa

550.0 °C

98 MPa

Show Material materials with Yield strength Rp0.2 of 98 MPa

Unlock all property charts

Yield strength Rp0.2, transverse

20.0 °C

240 MPa

Show Material materials with Yield strength Rp0.2, transverse of 240 MPa

Yield strength Rp1.0

20.0 °C

255 MPa

Show Material materials with Yield strength Rp1.0 of 255 MPa

100.0 °C

199 MPa

Show Material materials with Yield strength Rp1.0 of 199 MPa

150.0 °C

181 MPa

Show Material materials with Yield strength Rp1.0 of 181 MPa

200.0 °C

167 MPa

Show Material materials with Yield strength Rp1.0 of 167 MPa

250.0 °C

157 MPa

Show Material materials with Yield strength Rp1.0 of 157 MPa

300.0 °C

145 MPa

Show Material materials with Yield strength Rp1.0 of 145 MPa

350.0 °C

139 MPa

Show Material materials with Yield strength Rp1.0 of 139 MPa

400.0 °C

135 MPa

Show Material materials with Yield strength Rp1.0 of 135 MPa

450.0 °C

130 MPa

Show Material materials with Yield strength Rp1.0 of 130 MPa

500.0 °C

128 MPa

Show Material materials with Yield strength Rp1.0 of 128 MPa

550.0 °C

127 MPa

Show Material materials with Yield strength Rp1.0 of 127 MPa

Unlock all property charts

Yield strength Rp1.0, transverse

20.0 °C

270 MPa

Show Material materials with Yield strength Rp1.0, transverse of 270 MPa

Thermal

PropertyTemperatureValueComment

Coefficient of thermal expansion

-100.0 °C

1.49E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.49E-5 1/K

20.0 °C

1.61E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.61E-5 1/K

100.0 °C

1.65E-5 - 1.67E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.65E-5 - 1.67E-5 1/K

200.0 °C

1.72E-5 - 1.75E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.72E-5 - 1.75E-5 1/K

300.0 °C

1.75E-5 - 1.77E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.75E-5 - 1.77E-5 1/K

400.0 °C

1.81E-5 - 1.85E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.81E-5 - 1.85E-5 1/K

500.0 °C

1.84E-5 - 1.85E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.84E-5 - 1.85E-5 1/K

600.0 °C

1.88E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.88E-5 1/K

700.0 °C

1.91E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.91E-5 1/K

800.0 °C

1.94E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.94E-5 1/K

900.0 °C

1.97E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.97E-5 1/K

1000.0 °C

2E-5 1/K

Show Material materials with Coefficient of thermal expansion of 2E-5 1/K

Unlock all property charts

Melting point

1230 - 1480 °C

Show Material materials with Melting point of 1230 - 1480 °C

Typical for Austenitic Stainless Steel

Specific heat capacity

-100.0 °C

440 J/(kg·K)

Show Material materials with Specific heat capacity of 440 J/(kg·K)

20.0 °C

472 - 500 J/(kg·K)

Show Material materials with Specific heat capacity of 472 - 500 J/(kg·K)

100.0 °C

487 J/(kg·K)

Show Material materials with Specific heat capacity of 487 J/(kg·K)

200.0 °C

503 J/(kg·K)

Show Material materials with Specific heat capacity of 503 J/(kg·K)

300.0 °C

512 J/(kg·K)

Show Material materials with Specific heat capacity of 512 J/(kg·K)

400.0 °C

520 J/(kg·K)

Show Material materials with Specific heat capacity of 520 J/(kg·K)

500.0 °C

530 J/(kg·K)

Show Material materials with Specific heat capacity of 530 J/(kg·K)

600.0 °C

541 J/(kg·K)

Show Material materials with Specific heat capacity of 541 J/(kg·K)

700.0 °C

551 J/(kg·K)

Show Material materials with Specific heat capacity of 551 J/(kg·K)

800.0 °C

559 J/(kg·K)

Show Material materials with Specific heat capacity of 559 J/(kg·K)

900.0 °C

565 J/(kg·K)

Show Material materials with Specific heat capacity of 565 J/(kg·K)

1000.0 °C

571 J/(kg·K)

Show Material materials with Specific heat capacity of 571 J/(kg·K)

Unlock all property charts

Thermal conductivity

20.0 °C

13.3 - 15 W/(m·K)

Show Material materials with Thermal conductivity of 13.3 - 15 W/(m·K)

100.0 °C

14.9 W/(m·K)

Show Material materials with Thermal conductivity of 14.9 W/(m·K)

200.0 °C

16.5 W/(m·K)

Show Material materials with Thermal conductivity of 16.5 W/(m·K)

300.0 °C

18.1 W/(m·K)

Show Material materials with Thermal conductivity of 18.1 W/(m·K)

400.0 °C

19.5 W/(m·K)

Show Material materials with Thermal conductivity of 19.5 W/(m·K)

500.0 °C

21 W/(m·K)

Show Material materials with Thermal conductivity of 21 W/(m·K)

600.0 °C

22.4 W/(m·K)

Show Material materials with Thermal conductivity of 22.4 W/(m·K)

700.0 °C

23.8 W/(m·K)

Show Material materials with Thermal conductivity of 23.8 W/(m·K)

800.0 °C

25.2 W/(m·K)

Show Material materials with Thermal conductivity of 25.2 W/(m·K)

Unlock all property charts

Thermal diffusivity

20.0 °C

3.5 mm²/s

Show Material materials with Thermal diffusivity of 3.5 mm²/s

100.0 °C

3.8 mm²/s

Show Material materials with Thermal diffusivity of 3.8 mm²/s

200.0 °C

4 mm²/s

Show Material materials with Thermal diffusivity of 4 mm²/s

300.0 °C

4.3 mm²/s

Show Material materials with Thermal diffusivity of 4.3 mm²/s

400.0 °C

4.5 mm²/s

Show Material materials with Thermal diffusivity of 4.5 mm²/s

500.0 °C

4.7 mm²/s

Show Material materials with Thermal diffusivity of 4.7 mm²/s

600.0 °C

4.8 mm²/s

Show Material materials with Thermal diffusivity of 4.8 mm²/s

700.0 °C

5.1 mm²/s

Show Material materials with Thermal diffusivity of 5.1 mm²/s

800.0 °C

5.4 mm²/s

Show Material materials with Thermal diffusivity of 5.4 mm²/s

Unlock all property charts

Electrical

PropertyTemperatureValue

Electrical resistivity

20.0 °C

7.5E-7 - 7.91E-7 Ω·m

Show Material materials with Electrical resistivity of 7.5E-7 - 7.91E-7 Ω·m

100.0 °C

8.45E-7 Ω·m

Show Material materials with Electrical resistivity of 8.45E-7 Ω·m

200.0 °C

9.19E-7 Ω·m

Show Material materials with Electrical resistivity of 9.19E-7 Ω·m

300.0 °C

9.77E-7 Ω·m

Show Material materials with Electrical resistivity of 9.77E-7 Ω·m

400.0 °C

1.03E-6 Ω·m

Show Material materials with Electrical resistivity of 1.03E-6 Ω·m

500.0 °C

1.08E-6 Ω·m

Show Material materials with Electrical resistivity of 1.08E-6 Ω·m

600.0 °C

1.12E-6 Ω·m

Show Material materials with Electrical resistivity of 1.12E-6 Ω·m

700.0 °C

1.15E-6 Ω·m

Show Material materials with Electrical resistivity of 1.15E-6 Ω·m

800.0 °C

1.18E-6 Ω·m

Show Material materials with Electrical resistivity of 1.18E-6 Ω·m

Unlock all property charts

Chemical properties

PropertyValue

Carbon

0.03 %

Show Material materials with Carbon of 0.03 %

Chromium

16.5 - 18.5 %

Show Material materials with Chromium of 16.5 - 18.5 %

Manganese

2 %

Show Material materials with Manganese of 2 %

Molybdenum

2 - 2.5 %

Show Material materials with Molybdenum of 2 - 2.5 %

Nickel

10 - 13 %

Show Material materials with Nickel of 10 - 13 %

Nitrogen

0.11 %

Show Material materials with Nitrogen of 0.11 %

Phosphorus

0.05 %

Show Material materials with Phosphorus of 0.05 %

Silicon

1 %

Show Material materials with Silicon of 1 %

Sulfur

0.015 %

Show Material materials with Sulfur of 0.015 %