EN 10216-5 Grade X2CrNi18-9 solution annealed (+AT)

Want to keep this datasheet? Save it now in your required format

Description

The austenitic steel X2CrNi18-9 is available in solution annealed condition in the form of cold rolled strip, warm rolled strip and warm rolled sheet. The material is resistant to intercrystalline corrosion also in welded condition.

Related Standards

Equivalent Materials

This material data has been provided by WIAM.

All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

Ashby charts

See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Properties

General

PropertyTemperatureValue

Density

20.0 °C

7.9 g/cm³

Show Material materials with Density of 7.9 g/cm³

Mechanical

PropertyTemperatureValueComment

Elastic modulus

20.0 °C

200 GPa

Show Material materials with Elastic modulus of 200 GPa

100.0 °C

194 GPa

Show Material materials with Elastic modulus of 194 GPa

200.0 °C

186 GPa

Show Material materials with Elastic modulus of 186 GPa

300.0 °C

179 GPa

Show Material materials with Elastic modulus of 179 GPa

400.0 °C

172 GPa

Show Material materials with Elastic modulus of 172 GPa

500.0 °C

165 GPa

Show Material materials with Elastic modulus of 165 GPa

Elongation

20.0 °C

40 %

Show Material materials with Elongation of 40 %

Elongation, transverse

20.0 °C

35 %

Show Material materials with Elongation, transverse of 35 %

Poisson's ratio

23.0 °C

0.3 [-]

Show Material materials with Poisson's ratio of 0.3 [-]

Typical for Austenitic Stainless Steel

Shear modulus

23.0 °C

77 GPa

Show Material materials with Shear modulus of 77 GPa

Typical for Austenitic Stainless Steel

Tensile strength

20.0 °C

460 - 680 MPa

Show Material materials with Tensile strength of 460 - 680 MPa

Tensile strength, transverse

20.0 °C

460 - 680 MPa

Show Material materials with Tensile strength, transverse of 460 - 680 MPa

Yield strength Rp0.2

20.0 °C

180 MPa

Show Material materials with Yield strength Rp0.2 of 180 MPa

50.0 °C

165 MPa

Show Material materials with Yield strength Rp0.2 of 165 MPa

100.0 °C

145 MPa

Show Material materials with Yield strength Rp0.2 of 145 MPa

150.0 °C

130 MPa

Show Material materials with Yield strength Rp0.2 of 130 MPa

200.0 °C

118 MPa

Show Material materials with Yield strength Rp0.2 of 118 MPa

250.0 °C

108 MPa

Show Material materials with Yield strength Rp0.2 of 108 MPa

300.0 °C

100 MPa

Show Material materials with Yield strength Rp0.2 of 100 MPa

350.0 °C

94 MPa

Show Material materials with Yield strength Rp0.2 of 94 MPa

400.0 °C

89 MPa

Show Material materials with Yield strength Rp0.2 of 89 MPa

450.0 °C

85 MPa

Show Material materials with Yield strength Rp0.2 of 85 MPa

500.0 °C

81 MPa

Show Material materials with Yield strength Rp0.2 of 81 MPa

550.0 °C

80 MPa

Show Material materials with Yield strength Rp0.2 of 80 MPa

Unlock all property charts

Yield strength Rp0.2, transverse

20.0 °C

180 MPa

Show Material materials with Yield strength Rp0.2, transverse of 180 MPa

Yield strength Rp1.0

20.0 °C

215 MPa

Show Material materials with Yield strength Rp1.0 of 215 MPa

50.0 °C

200 MPa

Show Material materials with Yield strength Rp1.0 of 200 MPa

100.0 °C

180 MPa

Show Material materials with Yield strength Rp1.0 of 180 MPa

150.0 °C

160 MPa

Show Material materials with Yield strength Rp1.0 of 160 MPa

200.0 °C

145 MPa

Show Material materials with Yield strength Rp1.0 of 145 MPa

250.0 °C

135 MPa

Show Material materials with Yield strength Rp1.0 of 135 MPa

300.0 °C

127 MPa

Show Material materials with Yield strength Rp1.0 of 127 MPa

350.0 °C

121 MPa

Show Material materials with Yield strength Rp1.0 of 121 MPa

400.0 °C

116 MPa

Show Material materials with Yield strength Rp1.0 of 116 MPa

450.0 °C

112 MPa

Show Material materials with Yield strength Rp1.0 of 112 MPa

500.0 °C

109 MPa

Show Material materials with Yield strength Rp1.0 of 109 MPa

550.0 °C

108 MPa

Show Material materials with Yield strength Rp1.0 of 108 MPa

Unlock all property charts

Yield strength Rp1.0, transverse

20.0 °C

215 MPa

Show Material materials with Yield strength Rp1.0, transverse of 215 MPa

Thermal

PropertyTemperatureValueComment

Coefficient of thermal expansion

100.0 °C

1.6E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.6E-5 1/K

200.0 °C

1.65E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.65E-5 1/K

300.0 °C

1.7E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.7E-5 1/K

400.0 °C

1.8E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.8E-5 1/K

500.0 °C

1.8E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.8E-5 1/K

Unlock all property charts

Melting point

1230 - 1480 °C

Show Material materials with Melting point of 1230 - 1480 °C

Typical for Austenitic Stainless Steel

Specific heat capacity

20.0 °C

500 J/(kg·K)

Show Material materials with Specific heat capacity of 500 J/(kg·K)

Thermal conductivity

20.0 °C

15 W/(m·K)

Show Material materials with Thermal conductivity of 15 W/(m·K)

Electrical

PropertyTemperatureValue

Electrical resistivity

20.0 °C

7.3E-7 Ω·m

Show Material materials with Electrical resistivity of 7.3E-7 Ω·m

Chemical properties

PropertyValue

Carbon

0.03 %

Show Material materials with Carbon of 0.03 %

Chromium

17.5 - 19.5 %

Show Material materials with Chromium of 17.5 - 19.5 %

Manganese

2 %

Show Material materials with Manganese of 2 %

Nickel

8 - 10 %

Show Material materials with Nickel of 8 - 10 %

Nitrogen

0.1 - 0.11 %

Show Material materials with Nitrogen of 0.1 - 0.11 %

Phosphorus

0.04 %

Show Material materials with Phosphorus of 0.04 %

Silicon

1 %

Show Material materials with Silicon of 1 %

Sulfur

0.015 %

Show Material materials with Sulfur of 0.015 %