EN 10217-7 Grade X5CrNiMo17-12-2 solution annealed (+AT)

Want to keep this datasheet? Save it now in your required format

Description

The austenitic steel X5CrNiMo17-12-2 is available in the solution annealed condition. Welded circular tubes of this steel are used for compression load and for corrosive load at room temperature, low temperatures and elevated temperatures. The material is resistant to intercrystalline corrosion (up to 300 °C) also in the welded condition.

Related Standards

Equivalent Materials

This material data has been provided by WIAM.

All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

Ashby charts

See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Properties

General

PropertyTemperatureValue

Density

20.0 °C

7.96 - 8 g/cm³

Show Material materials with Density of 7.96 - 8 g/cm³

22.0 °C

7.96 g/cm³

Show Material materials with Density of 7.96 g/cm³

Mechanical

PropertyTemperatureValue

Elastic modulus

-100.0 °C

206 GPa

Show Material materials with Elastic modulus of 206 GPa

20.0 °C

196 - 200 GPa

Show Material materials with Elastic modulus of 196 - 200 GPa

22.0 °C

196.2 GPa

Show Material materials with Elastic modulus of 196.2 GPa

24.0 °C

193.1 - 197.9 GPa

Show Material materials with Elastic modulus of 193.1 - 197.9 GPa

100.0 °C

190 - 194 GPa

Show Material materials with Elastic modulus of 190 - 194 GPa

149.0 °C

184.8 - 190.3 GPa

Show Material materials with Elastic modulus of 184.8 - 190.3 GPa

200.0 °C

182 - 186 GPa

Show Material materials with Elastic modulus of 182 - 186 GPa

260.0 °C

182 - 182.7 GPa

Show Material materials with Elastic modulus of 182 - 182.7 GPa

300.0 °C

174 - 179 GPa

Show Material materials with Elastic modulus of 174 - 179 GPa

371.0 °C

174.4 - 179.3 GPa

Show Material materials with Elastic modulus of 174.4 - 179.3 GPa

400.0 °C

166 - 172 GPa

Show Material materials with Elastic modulus of 166 - 172 GPa

483.0 °C

163.4 - 165.5 GPa

Show Material materials with Elastic modulus of 163.4 - 165.5 GPa

500.0 °C

158 - 165 GPa

Show Material materials with Elastic modulus of 158 - 165 GPa

593.0 °C

153.4 - 157.9 GPa

Show Material materials with Elastic modulus of 153.4 - 157.9 GPa

600.0 °C

150 GPa

Show Material materials with Elastic modulus of 150 GPa

700.0 °C

142 GPa

Show Material materials with Elastic modulus of 142 GPa

704.0 °C

143.4 - 146.2 GPa

Show Material materials with Elastic modulus of 143.4 - 146.2 GPa

800.0 °C

134 GPa

Show Material materials with Elastic modulus of 134 GPa

816.0 °C

124.1 - 133.1 GPa

Show Material materials with Elastic modulus of 124.1 - 133.1 GPa

900.0 °C

127 GPa

Show Material materials with Elastic modulus of 127 GPa

1000.0 °C

120 GPa

Show Material materials with Elastic modulus of 120 GPa

Unlock all property charts

Elongation

20.0 °C

40 %

Show Material materials with Elongation of 40 %

Elongation, transverse

20.0 °C

30 %

Show Material materials with Elongation, transverse of 30 %

Poisson's ratio

22.0 °C

0.29 [-]

Show Material materials with Poisson's ratio of 0.29 [-]

24.0 °C

0.23 - 0.28 [-]

Show Material materials with Poisson's ratio of 0.23 - 0.28 [-]

149.0 °C

0.24 - 0.28 [-]

Show Material materials with Poisson's ratio of 0.24 - 0.28 [-]

260.0 °C

0.28 - 0.31 [-]

Show Material materials with Poisson's ratio of 0.28 - 0.31 [-]

371.0 °C

0.33 - 0.36 [-]

Show Material materials with Poisson's ratio of 0.33 - 0.36 [-]

483.0 °C

0.29 - 0.32 [-]

Show Material materials with Poisson's ratio of 0.29 - 0.32 [-]

593.0 °C

0.32 [-]

Show Material materials with Poisson's ratio of 0.32 [-]

704.0 °C

0.28 - 0.34 [-]

Show Material materials with Poisson's ratio of 0.28 - 0.34 [-]

816.0 °C

0.22 - 0.27 [-]

Show Material materials with Poisson's ratio of 0.22 - 0.27 [-]

Unlock all property charts

Shear modulus

22.0 °C

75.8 GPa

Show Material materials with Shear modulus of 75.8 GPa

24.0 °C

77.2 - 78.6 GPa

Show Material materials with Shear modulus of 77.2 - 78.6 GPa

149.0 °C

74.5 GPa

Show Material materials with Shear modulus of 74.5 GPa

260.0 °C

69.6 - 71 GPa

Show Material materials with Shear modulus of 69.6 - 71 GPa

371.0 °C

64.1 - 67.6 GPa

Show Material materials with Shear modulus of 64.1 - 67.6 GPa

483.0 °C

62.1 - 64.1 GPa

Show Material materials with Shear modulus of 62.1 - 64.1 GPa

593.0 °C

57.9 - 60 GPa

Show Material materials with Shear modulus of 57.9 - 60 GPa

704.0 °C

54.5 - 55.9 GPa

Show Material materials with Shear modulus of 54.5 - 55.9 GPa

816.0 °C

51 - 52.4 GPa

Show Material materials with Shear modulus of 51 - 52.4 GPa

Unlock all property charts

Tensile strength

20.0 °C

510 - 710 MPa

Show Material materials with Tensile strength of 510 - 710 MPa

Tensile strength, transverse

20.0 °C

510 - 710 MPa

Show Material materials with Tensile strength, transverse of 510 - 710 MPa

Yield strength Rp0.2

20.0 °C

205 MPa

Show Material materials with Yield strength Rp0.2 of 205 MPa

50.0 °C

196 MPa

Show Material materials with Yield strength Rp0.2 of 196 MPa

100.0 °C

175 MPa

Show Material materials with Yield strength Rp0.2 of 175 MPa

150.0 °C

158 MPa

Show Material materials with Yield strength Rp0.2 of 158 MPa

200.0 °C

145 MPa

Show Material materials with Yield strength Rp0.2 of 145 MPa

250.0 °C

135 MPa

Show Material materials with Yield strength Rp0.2 of 135 MPa

300.0 °C

127 MPa

Show Material materials with Yield strength Rp0.2 of 127 MPa

350.0 °C

120 MPa

Show Material materials with Yield strength Rp0.2 of 120 MPa

400.0 °C

115 MPa

Show Material materials with Yield strength Rp0.2 of 115 MPa

450.0 °C

112 MPa

Show Material materials with Yield strength Rp0.2 of 112 MPa

500.0 °C

110 MPa

Show Material materials with Yield strength Rp0.2 of 110 MPa

550.0 °C

108 MPa

Show Material materials with Yield strength Rp0.2 of 108 MPa

Unlock all property charts

Yield strength Rp0.2, transverse

20.0 °C

205 MPa

Show Material materials with Yield strength Rp0.2, transverse of 205 MPa

Yield strength Rp1.0

20.0 °C

240 MPa

Show Material materials with Yield strength Rp1.0 of 240 MPa

50.0 °C

230 MPa

Show Material materials with Yield strength Rp1.0 of 230 MPa

100.0 °C

210 MPa

Show Material materials with Yield strength Rp1.0 of 210 MPa

150.0 °C

190 MPa

Show Material materials with Yield strength Rp1.0 of 190 MPa

200.0 °C

175 MPa

Show Material materials with Yield strength Rp1.0 of 175 MPa

250.0 °C

165 MPa

Show Material materials with Yield strength Rp1.0 of 165 MPa

300.0 °C

155 MPa

Show Material materials with Yield strength Rp1.0 of 155 MPa

350.0 °C

150 MPa

Show Material materials with Yield strength Rp1.0 of 150 MPa

400.0 °C

145 MPa

Show Material materials with Yield strength Rp1.0 of 145 MPa

450.0 °C

141 MPa

Show Material materials with Yield strength Rp1.0 of 141 MPa

500.0 °C

139 MPa

Show Material materials with Yield strength Rp1.0 of 139 MPa

550.0 °C

137 MPa

Show Material materials with Yield strength Rp1.0 of 137 MPa

Unlock all property charts

Thermal

PropertyTemperatureValueComment

Coefficient of thermal expansion

-100.0 °C

1.49E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.49E-5 1/K

20.0 °C

1.61E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.61E-5 1/K

100.0 °C

1.6E-5 - 1.67E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.6E-5 - 1.67E-5 1/K

200.0 °C

1.65E-5 - 1.72E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.65E-5 - 1.72E-5 1/K

300.0 °C

1.7E-5 - 1.77E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.7E-5 - 1.77E-5 1/K

400.0 °C

1.75E-5 - 1.81E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.75E-5 - 1.81E-5 1/K

500.0 °C

1.8E-5 - 1.84E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.8E-5 - 1.84E-5 1/K

600.0 °C

1.88E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.88E-5 1/K

700.0 °C

1.91E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.91E-5 1/K

800.0 °C

1.94E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.94E-5 1/K

900.0 °C

1.97E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.97E-5 1/K

1000.0 °C

2E-5 1/K

Show Material materials with Coefficient of thermal expansion of 2E-5 1/K

Unlock all property charts

Melting point

1230 - 1480 °C

Show Material materials with Melting point of 1230 - 1480 °C

Typical for Austenitic Stainless Steel

Specific heat capacity

-100.0 °C

440 J/(kg·K)

Show Material materials with Specific heat capacity of 440 J/(kg·K)

20.0 °C

472 - 500 J/(kg·K)

Show Material materials with Specific heat capacity of 472 - 500 J/(kg·K)

100.0 °C

487 J/(kg·K)

Show Material materials with Specific heat capacity of 487 J/(kg·K)

200.0 °C

503 J/(kg·K)

Show Material materials with Specific heat capacity of 503 J/(kg·K)

300.0 °C

512 J/(kg·K)

Show Material materials with Specific heat capacity of 512 J/(kg·K)

400.0 °C

520 J/(kg·K)

Show Material materials with Specific heat capacity of 520 J/(kg·K)

500.0 °C

530 J/(kg·K)

Show Material materials with Specific heat capacity of 530 J/(kg·K)

600.0 °C

541 J/(kg·K)

Show Material materials with Specific heat capacity of 541 J/(kg·K)

700.0 °C

551 J/(kg·K)

Show Material materials with Specific heat capacity of 551 J/(kg·K)

800.0 °C

559 J/(kg·K)

Show Material materials with Specific heat capacity of 559 J/(kg·K)

900.0 °C

565 J/(kg·K)

Show Material materials with Specific heat capacity of 565 J/(kg·K)

1000.0 °C

571 J/(kg·K)

Show Material materials with Specific heat capacity of 571 J/(kg·K)

Unlock all property charts

Thermal conductivity

20.0 °C

13.3 - 15 W/(m·K)

Show Material materials with Thermal conductivity of 13.3 - 15 W/(m·K)

100.0 °C

14.9 W/(m·K)

Show Material materials with Thermal conductivity of 14.9 W/(m·K)

200.0 °C

16.5 W/(m·K)

Show Material materials with Thermal conductivity of 16.5 W/(m·K)

300.0 °C

18.1 W/(m·K)

Show Material materials with Thermal conductivity of 18.1 W/(m·K)

400.0 °C

19.5 W/(m·K)

Show Material materials with Thermal conductivity of 19.5 W/(m·K)

500.0 °C

21 W/(m·K)

Show Material materials with Thermal conductivity of 21 W/(m·K)

600.0 °C

22.4 W/(m·K)

Show Material materials with Thermal conductivity of 22.4 W/(m·K)

700.0 °C

23.8 W/(m·K)

Show Material materials with Thermal conductivity of 23.8 W/(m·K)

800.0 °C

25.2 W/(m·K)

Show Material materials with Thermal conductivity of 25.2 W/(m·K)

Unlock all property charts

Thermal diffusivity

20.0 °C

3.5 mm²/s

Show Material materials with Thermal diffusivity of 3.5 mm²/s

100.0 °C

3.8 mm²/s

Show Material materials with Thermal diffusivity of 3.8 mm²/s

200.0 °C

4 mm²/s

Show Material materials with Thermal diffusivity of 4 mm²/s

300.0 °C

4.3 mm²/s

Show Material materials with Thermal diffusivity of 4.3 mm²/s

400.0 °C

4.5 mm²/s

Show Material materials with Thermal diffusivity of 4.5 mm²/s

500.0 °C

4.7 mm²/s

Show Material materials with Thermal diffusivity of 4.7 mm²/s

600.0 °C

4.8 mm²/s

Show Material materials with Thermal diffusivity of 4.8 mm²/s

700.0 °C

5.1 mm²/s

Show Material materials with Thermal diffusivity of 5.1 mm²/s

800.0 °C

5.4 mm²/s

Show Material materials with Thermal diffusivity of 5.4 mm²/s

Unlock all property charts

Electrical

PropertyTemperatureValue

Electrical resistivity

20.0 °C

7.5E-7 - 7.91E-7 Ω·m

Show Material materials with Electrical resistivity of 7.5E-7 - 7.91E-7 Ω·m

100.0 °C

8.45E-7 Ω·m

Show Material materials with Electrical resistivity of 8.45E-7 Ω·m

200.0 °C

9.19E-7 Ω·m

Show Material materials with Electrical resistivity of 9.19E-7 Ω·m

300.0 °C

9.77E-7 Ω·m

Show Material materials with Electrical resistivity of 9.77E-7 Ω·m

400.0 °C

1.03E-6 Ω·m

Show Material materials with Electrical resistivity of 1.03E-6 Ω·m

500.0 °C

1.08E-6 Ω·m

Show Material materials with Electrical resistivity of 1.08E-6 Ω·m

600.0 °C

1.12E-6 Ω·m

Show Material materials with Electrical resistivity of 1.12E-6 Ω·m

700.0 °C

1.15E-6 Ω·m

Show Material materials with Electrical resistivity of 1.15E-6 Ω·m

800.0 °C

1.18E-6 Ω·m

Show Material materials with Electrical resistivity of 1.18E-6 Ω·m

Unlock all property charts

Chemical properties

PropertyValue

Carbon

0.07 %

Show Material materials with Carbon of 0.07 %

Chromium

16.5 - 18.5 %

Show Material materials with Chromium of 16.5 - 18.5 %

Manganese

2 %

Show Material materials with Manganese of 2 %

Molybdenum

2 - 2.5 %

Show Material materials with Molybdenum of 2 - 2.5 %

Nickel

10 - 13 %

Show Material materials with Nickel of 10 - 13 %

Nitrogen

0.11 %

Show Material materials with Nitrogen of 0.11 %

Phosphorus

0.05 %

Show Material materials with Phosphorus of 0.05 %

Silicon

1 %

Show Material materials with Silicon of 1 %

Sulfur

0.015 %

Show Material materials with Sulfur of 0.015 %