High-temperature steel with thermal resistance up to 580 °C for temperature loaded components, for screws and nuts. Further application for mounting elements at increased temperatures.

Related Standards

Equivalent Materials

This material data has been provided by WIAM.

All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

Ashby charts

See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Properties

General

PropertyTemperatureValue

Density

20.0 °C

7.7 - 7.76 g/cm³

Show Material materials with Density of 7.7 - 7.76 g/cm³

Mechanical

PropertyTemperatureValue

Elastic modulus

20.0 °C

216 - 218 GPa

Show Material materials with Elastic modulus of 216 - 218 GPa

100.0 °C

209 - 213 GPa

Show Material materials with Elastic modulus of 209 - 213 GPa

200.0 °C

200 - 206 GPa

Show Material materials with Elastic modulus of 200 - 206 GPa

300.0 °C

190 - 198 GPa

Show Material materials with Elastic modulus of 190 - 198 GPa

400.0 °C

179 - 190 GPa

Show Material materials with Elastic modulus of 179 - 190 GPa

500.0 °C

167 - 180 GPa

Show Material materials with Elastic modulus of 167 - 180 GPa

600.0 °C

127 - 167 GPa

Show Material materials with Elastic modulus of 127 - 167 GPa

Hardness, Brinell

20.0 °C

302 [-]

Show Material materials with Hardness, Brinell of 302 [-]

Poisson's ratio

20.0 °C

0.28 [-]

Show Material materials with Poisson's ratio of 0.28 [-]

Shear modulus

20.0 °C

84.95 GPa

Show Material materials with Shear modulus of 84.95 GPa

Thermal

PropertyTemperatureValueComment

Coefficient of thermal expansion

20.0 °C

1.02E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.02E-5 1/K

100.0 °C

1.05E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.05E-5 1/K

200.0 °C

1.09E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.09E-5 1/K

300.0 °C

1.13E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.13E-5 1/K

400.0 °C

1.16E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.16E-5 1/K

500.0 °C

1.2E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.2E-5 1/K

600.0 °C

1.22E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.22E-5 1/K

Unlock all property charts

Max service temperature, long

0 - 580 °C

Show Material materials with Max service temperature, long of 0 - 580 °C

Melting point

1370 - 1530 °C

Show Material materials with Melting point of 1370 - 1530 °C

Typical for Martensitic Stainless Steel

Specific heat capacity

20.0 °C

439 J/(kg·K)

Show Material materials with Specific heat capacity of 439 J/(kg·K)

100.0 °C

474 J/(kg·K)

Show Material materials with Specific heat capacity of 474 J/(kg·K)

200.0 °C

498 J/(kg·K)

Show Material materials with Specific heat capacity of 498 J/(kg·K)

300.0 °C

517 J/(kg·K)

Show Material materials with Specific heat capacity of 517 J/(kg·K)

400.0 °C

538 J/(kg·K)

Show Material materials with Specific heat capacity of 538 J/(kg·K)

500.0 °C

564 J/(kg·K)

Show Material materials with Specific heat capacity of 564 J/(kg·K)

600.0 °C

598 J/(kg·K)

Show Material materials with Specific heat capacity of 598 J/(kg·K)

Unlock all property charts

Thermal conductivity

20.0 °C

24 W/(m·K)

Show Material materials with Thermal conductivity of 24 W/(m·K)

100.0 °C

24.4 W/(m·K)

Show Material materials with Thermal conductivity of 24.4 W/(m·K)

200.0 °C

24.8 W/(m·K)

Show Material materials with Thermal conductivity of 24.8 W/(m·K)

300.0 °C

25.1 W/(m·K)

Show Material materials with Thermal conductivity of 25.1 W/(m·K)

400.0 °C

25.6 W/(m·K)

Show Material materials with Thermal conductivity of 25.6 W/(m·K)

500.0 °C

26.1 W/(m·K)

Show Material materials with Thermal conductivity of 26.1 W/(m·K)

600.0 °C

26.4 W/(m·K)

Show Material materials with Thermal conductivity of 26.4 W/(m·K)

Unlock all property charts

Thermal diffusivity

20.0 °C

7.1 mm²/s

Show Material materials with Thermal diffusivity of 7.1 mm²/s

100.0 °C

6.3 mm²/s

Show Material materials with Thermal diffusivity of 6.3 mm²/s

200.0 °C

6 mm²/s

Show Material materials with Thermal diffusivity of 6 mm²/s

300.0 °C

5.7 mm²/s

Show Material materials with Thermal diffusivity of 5.7 mm²/s

400.0 °C

5.4 mm²/s

Show Material materials with Thermal diffusivity of 5.4 mm²/s

500.0 °C

4.9 mm²/s

Show Material materials with Thermal diffusivity of 4.9 mm²/s

600.0 °C

4.1 mm²/s

Show Material materials with Thermal diffusivity of 4.1 mm²/s

Unlock all property charts

Electrical

PropertyTemperatureValue

Electrical resistivity

20.0 °C

6.03E-7 Ω·m

Show Material materials with Electrical resistivity of 6.03E-7 Ω·m

100.0 °C

6.68E-7 Ω·m

Show Material materials with Electrical resistivity of 6.68E-7 Ω·m

200.0 °C

7.43E-7 Ω·m

Show Material materials with Electrical resistivity of 7.43E-7 Ω·m

300.0 °C

8.17E-7 Ω·m

Show Material materials with Electrical resistivity of 8.17E-7 Ω·m

400.0 °C

8.9E-7 Ω·m

Show Material materials with Electrical resistivity of 8.9E-7 Ω·m

500.0 °C

9.62E-7 Ω·m

Show Material materials with Electrical resistivity of 9.62E-7 Ω·m

600.0 °C

1.04E-6 Ω·m

Show Material materials with Electrical resistivity of 1.04E-6 Ω·m

Unlock all property charts

Chemical properties

PropertyValue

Aluminium

0.02 %

Show Material materials with Aluminium of 0.02 %

Boron

1.5E-3 - 2E-3 %

Show Material materials with Boron of 1.5E-3 - 2E-3 %

Carbon

0.17 - 0.23 %

Show Material materials with Carbon of 0.17 - 0.23 %

Chromium

10 - 11.5 %

Show Material materials with Chromium of 10 - 11.5 %

Manganese

0.4 - 0.9 %

Show Material materials with Manganese of 0.4 - 0.9 %

Molybdenum

0.5 - 0.8 %

Show Material materials with Molybdenum of 0.5 - 0.8 %

Nickel

0.2 - 0.6 %

Show Material materials with Nickel of 0.2 - 0.6 %

Niobium

0.25 - 0.55 %

Show Material materials with Niobium of 0.25 - 0.55 %

Nitrogen

0.05 - 0.1 %

Show Material materials with Nitrogen of 0.05 - 0.1 %

Phosphorus

0.03 %

Show Material materials with Phosphorus of 0.03 %

Silicon

0.5 %

Show Material materials with Silicon of 0.5 %

Sulfur

0.015 %

Show Material materials with Sulfur of 0.015 %

Vanadium

0.1 - 0.3 %

Show Material materials with Vanadium of 0.1 - 0.3 %