EN 10269 Grade X7CrNiMoBNb16-16 warm worked and precipitation hardened (+WW+P)

Want to keep this datasheet? Save it now in your required format

Description

Hardenable austenitic high-temperature steel with boron addition for an increase of thermal resistance and creep behavior as well as for neutron absorption. Thermal resistance up to 650 °C, scaling resistance up to 750 °C Application for screws and nuts, steam and gas turbines and in chemical industry for high-stress components, such as screws, shafts, spindles, valves, in reactor engineering. Further application for mounting elements at increased temperatures.

Related Standards

Equivalent Materials

This material data has been provided by WIAM.

All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

Ashby charts

See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Properties

General

PropertyTemperatureValue

Density

20.0 °C

7.9 - 8.01 g/cm³

Show Material materials with Density of 7.9 - 8.01 g/cm³

Mechanical

PropertyTemperatureValue

Elastic modulus

-100.0 °C

206 GPa

Show Material materials with Elastic modulus of 206 GPa

20.0 °C

196 - 197.57 GPa

Show Material materials with Elastic modulus of 196 - 197.57 GPa

100.0 °C

190 - 192 GPa

Show Material materials with Elastic modulus of 190 - 192 GPa

200.0 °C

182 - 186 GPa

Show Material materials with Elastic modulus of 182 - 186 GPa

300.0 °C

174 - 181 GPa

Show Material materials with Elastic modulus of 174 - 181 GPa

400.0 °C

166 - 174 GPa

Show Material materials with Elastic modulus of 166 - 174 GPa

500.0 °C

158 - 165 GPa

Show Material materials with Elastic modulus of 158 - 165 GPa

600.0 °C

150 - 157 GPa

Show Material materials with Elastic modulus of 150 - 157 GPa

700.0 °C

142 - 147 GPa

Show Material materials with Elastic modulus of 142 - 147 GPa

800.0 °C

134 GPa

Show Material materials with Elastic modulus of 134 GPa

Elongation

20.0 °C

16 %

Show Material materials with Elongation of 16 %

Poisson's ratio

20.0 °C

0.28 [-]

Show Material materials with Poisson's ratio of 0.28 [-]

Shear modulus

20.0 °C

77.3 GPa

Show Material materials with Shear modulus of 77.3 GPa

Tensile strength

20.0 °C

650 - 850 MPa

Show Material materials with Tensile strength of 650 - 850 MPa

50.0 °C

635 MPa

Show Material materials with Tensile strength of 635 MPa

100.0 °C

615 MPa

Show Material materials with Tensile strength of 615 MPa

150.0 °C

590 MPa

Show Material materials with Tensile strength of 590 MPa

200.0 °C

570 MPa

Show Material materials with Tensile strength of 570 MPa

250.0 °C

550 MPa

Show Material materials with Tensile strength of 550 MPa

300.0 °C

530 MPa

Show Material materials with Tensile strength of 530 MPa

350.0 °C

505 MPa

Show Material materials with Tensile strength of 505 MPa

400.0 °C

485 MPa

Show Material materials with Tensile strength of 485 MPa

450.0 °C

460 MPa

Show Material materials with Tensile strength of 460 MPa

500.0 °C

440 MPa

Show Material materials with Tensile strength of 440 MPa

550.0 °C

420 MPa

Show Material materials with Tensile strength of 420 MPa

600.0 °C

395 MPa

Show Material materials with Tensile strength of 395 MPa

650.0 °C

375 MPa

Show Material materials with Tensile strength of 375 MPa

Unlock all property charts

Yield strength Rp0.2

20.0 °C

500 MPa

Show Material materials with Yield strength Rp0.2 of 500 MPa

50.0 °C

489 MPa

Show Material materials with Yield strength Rp0.2 of 489 MPa

100.0 °C

470 MPa

Show Material materials with Yield strength Rp0.2 of 470 MPa

150.0 °C

451 MPa

Show Material materials with Yield strength Rp0.2 of 451 MPa

200.0 °C

432 MPa

Show Material materials with Yield strength Rp0.2 of 432 MPa

250.0 °C

412 MPa

Show Material materials with Yield strength Rp0.2 of 412 MPa

300.0 °C

393 MPa

Show Material materials with Yield strength Rp0.2 of 393 MPa

350.0 °C

372 MPa

Show Material materials with Yield strength Rp0.2 of 372 MPa

400.0 °C

353 MPa

Show Material materials with Yield strength Rp0.2 of 353 MPa

450.0 °C

334 MPa

Show Material materials with Yield strength Rp0.2 of 334 MPa

500.0 °C

314 MPa

Show Material materials with Yield strength Rp0.2 of 314 MPa

550.0 °C

284 MPa

Show Material materials with Yield strength Rp0.2 of 284 MPa

600.0 °C

255 MPa

Show Material materials with Yield strength Rp0.2 of 255 MPa

650.0 °C

206 MPa

Show Material materials with Yield strength Rp0.2 of 206 MPa

Unlock all property charts

Thermal

PropertyTemperatureValueComment

Coefficient of thermal expansion

-100.0 °C

1.49E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.49E-5 1/K

20.0 °C

1.61E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.61E-5 1/K

100.0 °C

1.66E-5 - 1.67E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.66E-5 - 1.67E-5 1/K

200.0 °C

1.72E-5 - 1.77E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.72E-5 - 1.77E-5 1/K

300.0 °C

1.77E-5 - 1.79E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.77E-5 - 1.79E-5 1/K

400.0 °C

1.79E-5 - 1.81E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.79E-5 - 1.81E-5 1/K

500.0 °C

1.79E-5 - 1.84E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.79E-5 - 1.84E-5 1/K

600.0 °C

1.81E-5 - 1.88E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.81E-5 - 1.88E-5 1/K

700.0 °C

1.91E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.91E-5 1/K

800.0 °C

1.94E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.94E-5 1/K

900.0 °C

1.97E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.97E-5 1/K

1000.0 °C

2E-5 1/K

Show Material materials with Coefficient of thermal expansion of 2E-5 1/K

Unlock all property charts

Max service temperature, long

0 - 750 °C

Show Material materials with Max service temperature, long of 0 - 750 °C

Melting point

1230 - 1480 °C

Show Material materials with Melting point of 1230 - 1480 °C

Typical for Austenitic Stainless Steel

Specific heat capacity

-100.0 °C

440 J/(kg·K)

Show Material materials with Specific heat capacity of 440 J/(kg·K)

20.0 °C

460 - 472 J/(kg·K)

Show Material materials with Specific heat capacity of 460 - 472 J/(kg·K)

100.0 °C

487 J/(kg·K)

Show Material materials with Specific heat capacity of 487 J/(kg·K)

200.0 °C

503 J/(kg·K)

Show Material materials with Specific heat capacity of 503 J/(kg·K)

300.0 °C

512 J/(kg·K)

Show Material materials with Specific heat capacity of 512 J/(kg·K)

400.0 °C

520 J/(kg·K)

Show Material materials with Specific heat capacity of 520 J/(kg·K)

500.0 °C

530 J/(kg·K)

Show Material materials with Specific heat capacity of 530 J/(kg·K)

600.0 °C

541 J/(kg·K)

Show Material materials with Specific heat capacity of 541 J/(kg·K)

700.0 °C

551 J/(kg·K)

Show Material materials with Specific heat capacity of 551 J/(kg·K)

800.0 °C

559 J/(kg·K)

Show Material materials with Specific heat capacity of 559 J/(kg·K)

900.0 °C

565 J/(kg·K)

Show Material materials with Specific heat capacity of 565 J/(kg·K)

1000.0 °C

571 J/(kg·K)

Show Material materials with Specific heat capacity of 571 J/(kg·K)

Unlock all property charts

Thermal conductivity

20.0 °C

13.5 - 15 W/(m·K)

Show Material materials with Thermal conductivity of 13.5 - 15 W/(m·K)

100.0 °C

14.9 W/(m·K)

Show Material materials with Thermal conductivity of 14.9 W/(m·K)

200.0 °C

16.7 W/(m·K)

Show Material materials with Thermal conductivity of 16.7 W/(m·K)

300.0 °C

18.3 W/(m·K)

Show Material materials with Thermal conductivity of 18.3 W/(m·K)

400.0 °C

19.8 W/(m·K)

Show Material materials with Thermal conductivity of 19.8 W/(m·K)

500.0 °C

21.3 W/(m·K)

Show Material materials with Thermal conductivity of 21.3 W/(m·K)

600.0 °C

22.7 W/(m·K)

Show Material materials with Thermal conductivity of 22.7 W/(m·K)

700.0 °C

24.2 W/(m·K)

Show Material materials with Thermal conductivity of 24.2 W/(m·K)

800.0 °C

25.6 W/(m·K)

Show Material materials with Thermal conductivity of 25.6 W/(m·K)

Unlock all property charts

Thermal diffusivity

20.0 °C

3.6 mm²/s

Show Material materials with Thermal diffusivity of 3.6 mm²/s

100.0 °C

3.7 mm²/s

Show Material materials with Thermal diffusivity of 3.7 mm²/s

200.0 °C

4 mm²/s

Show Material materials with Thermal diffusivity of 4 mm²/s

300.0 °C

4.4 mm²/s

Show Material materials with Thermal diffusivity of 4.4 mm²/s

400.0 °C

4.6 mm²/s

Show Material materials with Thermal diffusivity of 4.6 mm²/s

500.0 °C

4.7 mm²/s

Show Material materials with Thermal diffusivity of 4.7 mm²/s

600.0 °C

4.9 mm²/s

Show Material materials with Thermal diffusivity of 4.9 mm²/s

700.0 °C

5.2 mm²/s

Show Material materials with Thermal diffusivity of 5.2 mm²/s

800.0 °C

5.5 mm²/s

Show Material materials with Thermal diffusivity of 5.5 mm²/s

Unlock all property charts

Electrical

PropertyTemperatureValue

Electrical resistivity

20.0 °C

7.75E-7 Ω·m

Show Material materials with Electrical resistivity of 7.75E-7 Ω·m

100.0 °C

8.42E-7 Ω·m

Show Material materials with Electrical resistivity of 8.42E-7 Ω·m

200.0 °C

9.04E-7 Ω·m

Show Material materials with Electrical resistivity of 9.04E-7 Ω·m

300.0 °C

9.62E-7 Ω·m

Show Material materials with Electrical resistivity of 9.62E-7 Ω·m

400.0 °C

1.01E-6 Ω·m

Show Material materials with Electrical resistivity of 1.01E-6 Ω·m

500.0 °C

1.06E-6 Ω·m

Show Material materials with Electrical resistivity of 1.06E-6 Ω·m

600.0 °C

1.1E-6 Ω·m

Show Material materials with Electrical resistivity of 1.1E-6 Ω·m

700.0 °C

1.13E-6 Ω·m

Show Material materials with Electrical resistivity of 1.13E-6 Ω·m

800.0 °C

1.16E-6 Ω·m

Show Material materials with Electrical resistivity of 1.16E-6 Ω·m

Unlock all property charts

Chemical properties

PropertyValue

Boron

0.05 - 0.1 %

Show Material materials with Boron of 0.05 - 0.1 %

Carbon

0.04 - 0.1 %

Show Material materials with Carbon of 0.04 - 0.1 %

Chromium

15.5 - 17.5 %

Show Material materials with Chromium of 15.5 - 17.5 %

Manganese

1.5 %

Show Material materials with Manganese of 1.5 %

Molybdenum

1.6 - 2 %

Show Material materials with Molybdenum of 1.6 - 2 %

Nickel

15.5 - 17.5 %

Show Material materials with Nickel of 15.5 - 17.5 %

Phosphorus

0.05 %

Show Material materials with Phosphorus of 0.05 %

Silicon

0.3 - 0.6 %

Show Material materials with Silicon of 0.3 - 0.6 %

Sulfur

0.015 - 0.03 %