EN 10132-4 Grade 75Ni8 quenched and tempered (+QT)

Want to keep this datasheet? Save it now in your required format

Description

The steel 75Ni8 is used as cold rolled strip for springs and special applications in thicknesses of up to 6 mm and as tempered cold strip in thicknesses from 0.30 to 3.00 mm.

Related Standards

Equivalent Materials

This material data has been provided by WIAM.

All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

Ashby charts

See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Properties

General

PropertyTemperatureValueComment

Density

23.0 °C

8.8 g/cm³

Show Material materials with Density of 8.8 g/cm³

Typical for Nickel Steel

Mechanical

PropertyTemperatureValueComment

Elastic modulus

23.0 °C

200 - 215 GPa

Show Material materials with Elastic modulus of 200 - 215 GPa

Typical for Nickel Steel

Hardness, Rockwell C

20.0 °C

38.5 - 52.5 [-]

Show Material materials with Hardness, Rockwell C of 38.5 - 52.5 [-]

Hardness, Vickers

20.0 °C

370 - 570 [-]

Show Material materials with Hardness, Vickers of 370 - 570 [-]

Poisson's ratio

23.0 °C

0.29 [-]

Show Material materials with Poisson's ratio of 0.29 [-]

Typical for Nickel Steel

Shear modulus

23.0 °C

76 GPa

Show Material materials with Shear modulus of 76 GPa

Typical for Nickel Steel

Tensile strength

20.0 °C

1200 - 1800 MPa

Show Material materials with Tensile strength of 1200 - 1800 MPa

Thermal

PropertyTemperatureValueComment

Melting point

1316 - 1595 °C

Show Material materials with Melting point of 1316 - 1595 °C

Typical for Nickel Steel

Specific heat capacity

23.0 °C

456 J/(kg·K)

Show Material materials with Specific heat capacity of 456 J/(kg·K)

Typical for Nickel Steel

Thermal conductivity

23.0 °C

10 - 50 W/(m·K)

Show Material materials with Thermal conductivity of 10 - 50 W/(m·K)

Typical for Nickel Steel

Chemical properties

PropertyValue

Carbon

0.72 - 0.78 %

Show Material materials with Carbon of 0.72 - 0.78 %

Chromium

0.15 %

Show Material materials with Chromium of 0.15 %

Manganese

0.3 - 0.5 %

Show Material materials with Manganese of 0.3 - 0.5 %

Molybdenum

0.1 %

Show Material materials with Molybdenum of 0.1 %

Nickel

1.8 - 2.1 %

Show Material materials with Nickel of 1.8 - 2.1 %

Phosphorus

0.03 %

Show Material materials with Phosphorus of 0.03 %

Silicon

0.15 - 0.35 %

Show Material materials with Silicon of 0.15 - 0.35 %

Sulfur

0.025 %

Show Material materials with Sulfur of 0.025 %