General
Property | Temperature | Value |
---|---|---|
Density | 20.0 °C | 7.81 g/cm³ Show Material materials with Density of 7.81 g/cm³ |
Mechanical
Property | Temperature | Value |
---|---|---|
Elastic modulus | -100.0 °C | 217 GPa Show Material materials with Elastic modulus of 217 GPa |
20.0 °C | 212 - 212.9 GPa Show Material materials with Elastic modulus of 212 - 212.9 GPa | |
100.0 °C | 207 - 208.11 GPa Show Material materials with Elastic modulus of 207 - 208.11 GPa | |
200.0 °C | 199 - 201.77 GPa Show Material materials with Elastic modulus of 199 - 201.77 GPa | |
300.0 °C | 192 - 194.97 GPa Show Material materials with Elastic modulus of 192 - 194.97 GPa | |
400.0 °C | 184 - 186.79 GPa Show Material materials with Elastic modulus of 184 - 186.79 GPa | |
500.0 °C | 175 - 177.82 GPa Show Material materials with Elastic modulus of 175 - 177.82 GPa | |
600.0 °C | 164 GPa Show Material materials with Elastic modulus of 164 GPa | |
Hardness, Rockwell C | 20.0 °C | 61 [-] Show Material materials with Hardness, Rockwell C of 61 [-] |
Hardness, Vickers | 20.0 °C | 720 [-] Show Material materials with Hardness, Vickers of 720 [-] |
Poisson's ratio | 20.0 °C | 0.28 [-] Show Material materials with Poisson's ratio of 0.28 [-] |
100.0 °C | 0.29 [-] Show Material materials with Poisson's ratio of 0.29 [-] | |
200.0 °C | 0.29 [-] Show Material materials with Poisson's ratio of 0.29 [-] | |
300.0 °C | 0.3 [-] Show Material materials with Poisson's ratio of 0.3 [-] | |
400.0 °C | 0.3 [-] Show Material materials with Poisson's ratio of 0.3 [-] | |
500.0 °C | 0.31 [-] Show Material materials with Poisson's ratio of 0.31 [-] | |
Shear modulus | 20.0 °C | 83.12 GPa Show Material materials with Shear modulus of 83.12 GPa |
100.0 °C | 80.96 GPa Show Material materials with Shear modulus of 80.96 GPa | |
200.0 °C | 78.33 GPa Show Material materials with Shear modulus of 78.33 GPa | |
300.0 °C | 75.24 GPa Show Material materials with Shear modulus of 75.24 GPa | |
400.0 °C | 72 GPa Show Material materials with Shear modulus of 72 GPa | |
500.0 °C | 68.13 GPa Show Material materials with Shear modulus of 68.13 GPa | |
Thermal
Property | Temperature | Value | Comment |
---|---|---|---|
Coefficient of thermal expansion | -100.0 °C | 1.05E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.05E-5 1/K | |
20.0 °C | 1.15E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.15E-5 1/K | ||
100.0 °C | 1.21E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.21E-5 1/K | ||
200.0 °C | 1.27E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.27E-5 1/K | ||
300.0 °C | 1.32E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.32E-5 1/K | ||
400.0 °C | 1.36E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.36E-5 1/K | ||
500.0 °C | 1.4E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.4E-5 1/K | ||
600.0 °C | 1.44E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.44E-5 1/K | ||
Melting point | 1370 - 1425 °C Show Material materials with Melting point of 1370 - 1425 °C | Typical for Tool And Machining Steel | |
Specific heat capacity | -100.0 °C | 423 J/(kg·K) Show Material materials with Specific heat capacity of 423 J/(kg·K) | |
20.0 °C | 461 J/(kg·K) Show Material materials with Specific heat capacity of 461 J/(kg·K) | ||
100.0 °C | 479 J/(kg·K) Show Material materials with Specific heat capacity of 479 J/(kg·K) | ||
200.0 °C | 499 J/(kg·K) Show Material materials with Specific heat capacity of 499 J/(kg·K) | ||
300.0 °C | 517 J/(kg·K) Show Material materials with Specific heat capacity of 517 J/(kg·K) | ||
400.0 °C | 536 J/(kg·K) Show Material materials with Specific heat capacity of 536 J/(kg·K) | ||
500.0 °C | 558 J/(kg·K) Show Material materials with Specific heat capacity of 558 J/(kg·K) | ||
600.0 °C | 587 J/(kg·K) Show Material materials with Specific heat capacity of 587 J/(kg·K) | ||
Thermal conductivity | 20.0 °C | 39.6 W/(m·K) Show Material materials with Thermal conductivity of 39.6 W/(m·K) | |
100.0 °C | 41.6 W/(m·K) Show Material materials with Thermal conductivity of 41.6 W/(m·K) | ||
200.0 °C | 41.8 W/(m·K) Show Material materials with Thermal conductivity of 41.8 W/(m·K) | ||
300.0 °C | 40.3 W/(m·K) Show Material materials with Thermal conductivity of 40.3 W/(m·K) | ||
400.0 °C | 38.2 W/(m·K) Show Material materials with Thermal conductivity of 38.2 W/(m·K) | ||
500.0 °C | 36 W/(m·K) Show Material materials with Thermal conductivity of 36 W/(m·K) | ||
600.0 °C | 33.6 W/(m·K) Show Material materials with Thermal conductivity of 33.6 W/(m·K) | ||
Thermal diffusivity | 20.0 °C | 11 mm²/s Show Material materials with Thermal diffusivity of 11 mm²/s | |
100.0 °C | 10.8 mm²/s Show Material materials with Thermal diffusivity of 10.8 mm²/s | ||
200.0 °C | 10.1 mm²/s Show Material materials with Thermal diffusivity of 10.1 mm²/s | ||
300.0 °C | 9.2 mm²/s Show Material materials with Thermal diffusivity of 9.2 mm²/s | ||
400.0 °C | 8.1 mm²/s Show Material materials with Thermal diffusivity of 8.1 mm²/s | ||
500.0 °C | 7 mm²/s Show Material materials with Thermal diffusivity of 7 mm²/s | ||
600.0 °C | 5.7 mm²/s Show Material materials with Thermal diffusivity of 5.7 mm²/s | ||
Electrical
Property | Temperature | Value |
---|---|---|
Electrical resistivity | 20.0 °C | 2.63E-7 Ω·m Show Material materials with Electrical resistivity of 2.63E-7 Ω·m |
100.0 °C | 3.08E-7 Ω·m Show Material materials with Electrical resistivity of 3.08E-7 Ω·m | |
200.0 °C | 3.78E-7 Ω·m Show Material materials with Electrical resistivity of 3.78E-7 Ω·m | |
300.0 °C | 4.66E-7 Ω·m Show Material materials with Electrical resistivity of 4.66E-7 Ω·m | |
400.0 °C | 5.69E-7 Ω·m Show Material materials with Electrical resistivity of 5.69E-7 Ω·m | |
500.0 °C | 6.87E-7 Ω·m Show Material materials with Electrical resistivity of 6.87E-7 Ω·m | |
600.0 °C | 8.26E-7 Ω·m Show Material materials with Electrical resistivity of 8.26E-7 Ω·m | |
Chemical properties
Property | Value |
---|---|
Carbon | 0.95 - 1.1 % Show Material materials with Carbon of 0.95 - 1.1 % |
Chromium | 1.35 - 1.6 % Show Material materials with Chromium of 1.35 - 1.6 % |
Manganese | 0.2 - 0.4 % Show Material materials with Manganese of 0.2 - 0.4 % |
Molybdenum | 0.1 % Show Material materials with Molybdenum of 0.1 % |
Nickel | 0.4 % Show Material materials with Nickel of 0.4 % |
Phosphorus | 0.03 % Show Material materials with Phosphorus of 0.03 % |
Silicon | 0.15 - 0.35 % Show Material materials with Silicon of 0.15 - 0.35 % |
Sulfur | 0.025 % Show Material materials with Sulfur of 0.025 % |