EN 10250-4 Grade X3CrNiMo13-4 quenched and tempered (+QT)

Want to keep this datasheet? Save it now in your required format

Description

The make X3CrNiMo13-4 is comparable to X 4 CrNi 13 4 acc. to SEW 400: 1991-02. The steel shows at temperatures of -60 to 300 °C favorable ductility properties and sufficient corrosion resistance. Better corrosion qualities than comparable 13% Cr-steels due to the Ni-content. Application in tempered condition for turbine blade wheels, pumps, compressors, components of power plant and reactor construction as well as in shipbuilding.

Related Standards

Equivalent Materials

This material data has been provided by WIAM.

All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

Ashby charts

See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Properties

General

PropertyTemperatureValue

Density

20.0 °C

7.58 - 7.7 g/cm³

Show Material materials with Density of 7.58 - 7.7 g/cm³

Mechanical

PropertyTemperatureValueComment

Elastic modulus

20.0 °C

200 - 218 GPa

Show Material materials with Elastic modulus of 200 - 218 GPa

100.0 °C

195 - 213 GPa

Show Material materials with Elastic modulus of 195 - 213 GPa

200.0 °C

185 - 206 GPa

Show Material materials with Elastic modulus of 185 - 206 GPa

300.0 °C

175 - 198 GPa

Show Material materials with Elastic modulus of 175 - 198 GPa

400.0 °C

170 - 190 GPa

Show Material materials with Elastic modulus of 170 - 190 GPa

500.0 °C

180 GPa

Show Material materials with Elastic modulus of 180 GPa

600.0 °C

167 GPa

Show Material materials with Elastic modulus of 167 GPa

700.0 °C

150 GPa

Show Material materials with Elastic modulus of 150 GPa

Elongation

20.0 °C

12 - 15 %

Show Material materials with Elongation of 12 - 15 %

Elongation, transverse

20.0 °C

10 - 12 %

Show Material materials with Elongation, transverse of 10 - 12 %

Poisson's ratio

23.0 °C

0.3 [-]

Show Material materials with Poisson's ratio of 0.3 [-]

Typical for Martensitic Stainless Steel

Shear modulus

23.0 °C

77 GPa

Show Material materials with Shear modulus of 77 GPa

Typical for Martensitic Stainless Steel

Tensile strength

20.0 °C

650 - 1100 MPa

Show Material materials with Tensile strength of 650 - 1100 MPa

Tensile strength, transverse

20.0 °C

650 - 1100 MPa

Show Material materials with Tensile strength, transverse of 650 - 1100 MPa

Yield strength Rp0.2

20.0 °C

520 - 800 MPa

Show Material materials with Yield strength Rp0.2 of 520 - 800 MPa

100.0 °C

500 - 720 MPa

Show Material materials with Yield strength Rp0.2 of 500 - 720 MPa

150.0 °C

490 - 690 MPa

Show Material materials with Yield strength Rp0.2 of 490 - 690 MPa

200.0 °C

480 - 665 MPa

Show Material materials with Yield strength Rp0.2 of 480 - 665 MPa

250.0 °C

470 - 640 MPa

Show Material materials with Yield strength Rp0.2 of 470 - 640 MPa

300.0 °C

460 - 620 MPa

Show Material materials with Yield strength Rp0.2 of 460 - 620 MPa

350.0 °C

450 - 515 MPa

Show Material materials with Yield strength Rp0.2 of 450 - 515 MPa

Unlock all property charts

Thermal

PropertyTemperatureValueComment

Coefficient of thermal expansion

20.0 °C

1.02E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.02E-5 1/K

100.0 °C

1.05E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.05E-5 1/K

200.0 °C

1.09E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.09E-5 1/K

300.0 °C

1.13E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.13E-5 1/K

400.0 °C

1.16E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.16E-5 1/K

500.0 °C

1.2E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.2E-5 1/K

600.0 °C

1.22E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.22E-5 1/K

700.0 °C

1.24E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.24E-5 1/K

Unlock all property charts

Melting point

1370 - 1530 °C

Show Material materials with Melting point of 1370 - 1530 °C

Typical for Martensitic Stainless Steel

Specific heat capacity

20.0 °C

430 - 439 J/(kg·K)

Show Material materials with Specific heat capacity of 430 - 439 J/(kg·K)

100.0 °C

474 J/(kg·K)

Show Material materials with Specific heat capacity of 474 J/(kg·K)

200.0 °C

492 J/(kg·K)

Show Material materials with Specific heat capacity of 492 J/(kg·K)

300.0 °C

517 J/(kg·K)

Show Material materials with Specific heat capacity of 517 J/(kg·K)

400.0 °C

538 J/(kg·K)

Show Material materials with Specific heat capacity of 538 J/(kg·K)

500.0 °C

564 J/(kg·K)

Show Material materials with Specific heat capacity of 564 J/(kg·K)

600.0 °C

598 J/(kg·K)

Show Material materials with Specific heat capacity of 598 J/(kg·K)

700.0 °C

647 J/(kg·K)

Show Material materials with Specific heat capacity of 647 J/(kg·K)

Unlock all property charts

Thermal conductivity

20.0 °C

15.7 - 25 W/(m·K)

Show Material materials with Thermal conductivity of 15.7 - 25 W/(m·K)

100.0 °C

17.1 W/(m·K)

Show Material materials with Thermal conductivity of 17.1 W/(m·K)

200.0 °C

18.6 W/(m·K)

Show Material materials with Thermal conductivity of 18.6 W/(m·K)

300.0 °C

20 W/(m·K)

Show Material materials with Thermal conductivity of 20 W/(m·K)

400.0 °C

21.2 W/(m·K)

Show Material materials with Thermal conductivity of 21.2 W/(m·K)

500.0 °C

22.3 W/(m·K)

Show Material materials with Thermal conductivity of 22.3 W/(m·K)

600.0 °C

23.1 W/(m·K)

Show Material materials with Thermal conductivity of 23.1 W/(m·K)

700.0 °C

23.8 W/(m·K)

Show Material materials with Thermal conductivity of 23.8 W/(m·K)

Unlock all property charts

Thermal diffusivity

20.0 °C

4.7 mm²/s

Show Material materials with Thermal diffusivity of 4.7 mm²/s

100.0 °C

4.5 mm²/s

Show Material materials with Thermal diffusivity of 4.5 mm²/s

200.0 °C

4.6 mm²/s

Show Material materials with Thermal diffusivity of 4.6 mm²/s

300.0 °C

4.7 mm²/s

Show Material materials with Thermal diffusivity of 4.7 mm²/s

400.0 °C

4.5 mm²/s

Show Material materials with Thermal diffusivity of 4.5 mm²/s

500.0 °C

4.3 mm²/s

Show Material materials with Thermal diffusivity of 4.3 mm²/s

600.0 °C

3.7 mm²/s

Show Material materials with Thermal diffusivity of 3.7 mm²/s

700.0 °C

3 mm²/s

Show Material materials with Thermal diffusivity of 3 mm²/s

Unlock all property charts

Electrical

PropertyTemperatureValue

Electrical resistivity

20.0 °C

9.19E-7 Ω·m

Show Material materials with Electrical resistivity of 9.19E-7 Ω·m

100.0 °C

9.48E-7 Ω·m

Show Material materials with Electrical resistivity of 9.48E-7 Ω·m

200.0 °C

9.87E-7 Ω·m

Show Material materials with Electrical resistivity of 9.87E-7 Ω·m

300.0 °C

1.03E-6 Ω·m

Show Material materials with Electrical resistivity of 1.03E-6 Ω·m

400.0 °C

1.07E-6 Ω·m

Show Material materials with Electrical resistivity of 1.07E-6 Ω·m

500.0 °C

1.12E-6 Ω·m

Show Material materials with Electrical resistivity of 1.12E-6 Ω·m

600.0 °C

1.18E-6 Ω·m

Show Material materials with Electrical resistivity of 1.18E-6 Ω·m

700.0 °C

1.24E-6 Ω·m

Show Material materials with Electrical resistivity of 1.24E-6 Ω·m

Unlock all property charts

Chemical properties

PropertyValue

Carbon

0.05 %

Show Material materials with Carbon of 0.05 %

Chromium

12 - 14 %

Show Material materials with Chromium of 12 - 14 %

Manganese

1.5 %

Show Material materials with Manganese of 1.5 %

Molybdenum

0.3 - 0.7 %

Show Material materials with Molybdenum of 0.3 - 0.7 %

Nickel

3.5 - 4.5 %

Show Material materials with Nickel of 3.5 - 4.5 %

Nitrogen

0.02 %

Show Material materials with Nitrogen of 0.02 %

Phosphorus

0.04 %

Show Material materials with Phosphorus of 0.04 %

Silicon

0.7 %

Show Material materials with Silicon of 0.7 %

Sulfur

0.015 %

Show Material materials with Sulfur of 0.015 %