The stainless steel X7CrNiAl17-7 is usually used cold drawn as wire up to 10 mm diameter for springs or spring parts. It has a high fatigue strength and a raised high-temperature strength, but a reduced corrosion resistance and is applicable up to 300°C.

Related Standards

Equivalent Materials

This material data has been provided by WIAM.

All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

Ashby charts

See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Properties

General

PropertyTemperatureValue

Density

20.0 °C

7.92 g/cm³

Show Material materials with Density of 7.92 g/cm³

Mechanical

PropertyTemperatureValueComment

Elastic modulus

-100.0 °C

206 GPa

Show Material materials with Elastic modulus of 206 GPa

20.0 °C

190 - 200 GPa

Show Material materials with Elastic modulus of 190 - 200 GPa

100.0 °C

190 GPa

Show Material materials with Elastic modulus of 190 GPa

200.0 °C

182 GPa

Show Material materials with Elastic modulus of 182 GPa

300.0 °C

174 GPa

Show Material materials with Elastic modulus of 174 GPa

400.0 °C

166 GPa

Show Material materials with Elastic modulus of 166 GPa

500.0 °C

158 GPa

Show Material materials with Elastic modulus of 158 GPa

600.0 °C

150 GPa

Show Material materials with Elastic modulus of 150 GPa

700.0 °C

142 GPa

Show Material materials with Elastic modulus of 142 GPa

800.0 °C

134 GPa

Show Material materials with Elastic modulus of 134 GPa

Poisson's ratio

23.0 °C

0.3 [-]

Show Material materials with Poisson's ratio of 0.3 [-]

Typical for Steel

Shear modulus

20.0 °C

73 - 78 GPa

Show Material materials with Shear modulus of 73 - 78 GPa

Tensile strength

20.0 °C

1500 - 2275 MPa

Show Material materials with Tensile strength of 1500 - 2275 MPa

Thermal

PropertyTemperatureValue

Coefficient of thermal expansion

-100.0 °C

1.49E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.49E-5 1/K

20.0 °C

1.61E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.61E-5 1/K

100.0 °C

1.67E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.67E-5 1/K

200.0 °C

1.72E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.72E-5 1/K

300.0 °C

1.77E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.77E-5 1/K

400.0 °C

1.81E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.81E-5 1/K

500.0 °C

1.84E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.84E-5 1/K

600.0 °C

1.88E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.88E-5 1/K

700.0 °C

1.91E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.91E-5 1/K

800.0 °C

1.94E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.94E-5 1/K

Unlock all property charts

Max service temperature, long

-150 - 350 °C

Show Material materials with Max service temperature, long of -150 - 350 °C

Specific heat capacity

-100.0 °C

440 J/(kg·K)

Show Material materials with Specific heat capacity of 440 J/(kg·K)

20.0 °C

472 J/(kg·K)

Show Material materials with Specific heat capacity of 472 J/(kg·K)

100.0 °C

487 J/(kg·K)

Show Material materials with Specific heat capacity of 487 J/(kg·K)

200.0 °C

503 J/(kg·K)

Show Material materials with Specific heat capacity of 503 J/(kg·K)

300.0 °C

512 J/(kg·K)

Show Material materials with Specific heat capacity of 512 J/(kg·K)

400.0 °C

520 J/(kg·K)

Show Material materials with Specific heat capacity of 520 J/(kg·K)

500.0 °C

530 J/(kg·K)

Show Material materials with Specific heat capacity of 530 J/(kg·K)

600.0 °C

541 J/(kg·K)

Show Material materials with Specific heat capacity of 541 J/(kg·K)

700.0 °C

551 J/(kg·K)

Show Material materials with Specific heat capacity of 551 J/(kg·K)

800.0 °C

559 J/(kg·K)

Show Material materials with Specific heat capacity of 559 J/(kg·K)

Unlock all property charts

Thermal conductivity

-100.0 °C

11.7 W/(m·K)

Show Material materials with Thermal conductivity of 11.7 W/(m·K)

20.0 °C

14.5 W/(m·K)

Show Material materials with Thermal conductivity of 14.5 W/(m·K)

100.0 °C

16 W/(m·K)

Show Material materials with Thermal conductivity of 16 W/(m·K)

200.0 °C

17.6 W/(m·K)

Show Material materials with Thermal conductivity of 17.6 W/(m·K)

300.0 °C

19.1 W/(m·K)

Show Material materials with Thermal conductivity of 19.1 W/(m·K)

400.0 °C

20.4 W/(m·K)

Show Material materials with Thermal conductivity of 20.4 W/(m·K)

500.0 °C

21.9 W/(m·K)

Show Material materials with Thermal conductivity of 21.9 W/(m·K)

600.0 °C

23.3 W/(m·K)

Show Material materials with Thermal conductivity of 23.3 W/(m·K)

700.0 °C

24.7 W/(m·K)

Show Material materials with Thermal conductivity of 24.7 W/(m·K)

800.0 °C

26.1 W/(m·K)

Show Material materials with Thermal conductivity of 26.1 W/(m·K)

Unlock all property charts

Thermal diffusivity

-100.0 °C

3.7 mm²/s

Show Material materials with Thermal diffusivity of 3.7 mm²/s

20.0 °C

3.9 mm²/s

Show Material materials with Thermal diffusivity of 3.9 mm²/s

100.0 °C

4.3 mm²/s

Show Material materials with Thermal diffusivity of 4.3 mm²/s

200.0 °C

4.3 mm²/s

Show Material materials with Thermal diffusivity of 4.3 mm²/s

300.0 °C

4.6 mm²/s

Show Material materials with Thermal diffusivity of 4.6 mm²/s

400.0 °C

4.7 mm²/s

Show Material materials with Thermal diffusivity of 4.7 mm²/s

500.0 °C

4.9 mm²/s

Show Material materials with Thermal diffusivity of 4.9 mm²/s

600.0 °C

5 mm²/s

Show Material materials with Thermal diffusivity of 5 mm²/s

700.0 °C

5.3 mm²/s

Show Material materials with Thermal diffusivity of 5.3 mm²/s

800.0 °C

5.7 mm²/s

Show Material materials with Thermal diffusivity of 5.7 mm²/s

Unlock all property charts

Electrical

PropertyTemperatureValue

Electrical resistivity

-100.0 °C

5.86E-7 Ω·m

Show Material materials with Electrical resistivity of 5.86E-7 Ω·m

20.0 °C

6.92E-7 Ω·m

Show Material materials with Electrical resistivity of 6.92E-7 Ω·m

100.0 °C

7.58E-7 Ω·m

Show Material materials with Electrical resistivity of 7.58E-7 Ω·m

200.0 °C

8.36E-7 Ω·m

Show Material materials with Electrical resistivity of 8.36E-7 Ω·m

300.0 °C

9.07E-7 Ω·m

Show Material materials with Electrical resistivity of 9.07E-7 Ω·m

400.0 °C

9.73E-7 Ω·m

Show Material materials with Electrical resistivity of 9.73E-7 Ω·m

500.0 °C

1.02E-6 Ω·m

Show Material materials with Electrical resistivity of 1.02E-6 Ω·m

600.0 °C

1.06E-6 Ω·m

Show Material materials with Electrical resistivity of 1.06E-6 Ω·m

700.0 °C

1.1E-6 Ω·m

Show Material materials with Electrical resistivity of 1.1E-6 Ω·m

800.0 °C

1.13E-6 Ω·m

Show Material materials with Electrical resistivity of 1.13E-6 Ω·m

Unlock all property charts

Chemical properties

PropertyValue

Aluminium

0.7 - 1.5 %

Show Material materials with Aluminium of 0.7 - 1.5 %

Carbon

0.09 %

Show Material materials with Carbon of 0.09 %

Chromium

16 - 18 %

Show Material materials with Chromium of 16 - 18 %

Manganese

1 %

Show Material materials with Manganese of 1 %

Nickel

6.5 - 7.8 %

Show Material materials with Nickel of 6.5 - 7.8 %

Phosphorus

0.04 %

Show Material materials with Phosphorus of 0.04 %

Silicon

0.7 %

Show Material materials with Silicon of 0.7 %

Sulfur

0.015 %

Show Material materials with Sulfur of 0.015 %

Technological properties

Property
Features

Spring