General
Property | Temperature | Value |
---|---|---|
Density | 23.0 °C | 7.8 g/cm³ Show Material materials with Density of 7.8 g/cm³ |
Mechanical
Property | Temperature | Value | Comment |
---|---|---|---|
Elastic modulus | 23.0 °C | 220 GPa Show Material materials with Elastic modulus of 220 GPa | |
Elongation | 23.0 °C | 9.2 - 12 % Show Material materials with Elongation of 9.2 - 12 % | |
Poisson's ratio | 23.0 °C | 0.3 [-] Show Material materials with Poisson's ratio of 0.3 [-] | Typical for Steel |
Tensile strength | 23.0 °C | 1350 - 1510 MPa Show Material materials with Tensile strength of 1350 - 1510 MPa | |
Yield strength | 23.0 °C | 1190 - 1350 MPa Show Material materials with Yield strength of 1190 - 1350 MPa |
Thermal
Property | Temperature | Value |
---|---|---|
Coefficient of thermal expansion | 23.0 °C | 1.2E-5 1/K Show Material materials with Coefficient of thermal expansion of 1.2E-5 1/K |
Specific heat capacity | 23.0 °C | 450 J/(kg·K) Show Material materials with Specific heat capacity of 450 J/(kg·K) |
Chemical properties
Property | Value |
---|---|
Aluminium | 0 - 0.4 % Show Material materials with Aluminium of 0 - 0.4 % |
Carbon | 0 - 0.08 % Show Material materials with Carbon of 0 - 0.08 % |
Chromium | 16 - 17.5 % Show Material materials with Chromium of 16 - 17.5 % |
Iron | 71.3 - 77.6 % Show Material materials with Iron of 71.3 - 77.6 % |
Manganese | 0 - 1 % Show Material materials with Manganese of 0 - 1 % |
Nickel | 6 - 7.5 % Show Material materials with Nickel of 6 - 7.5 % |
Phosphorus | 0 - 0.04 % Show Material materials with Phosphorus of 0 - 0.04 % |
Silicon | 0 - 1 % Show Material materials with Silicon of 0 - 1 % |
Sulfur | 0 - 0.03 % Show Material materials with Sulfur of 0 - 0.03 % |
Titanium | 0.4 - 1.2 % Show Material materials with Titanium of 0.4 - 1.2 % |