EN 10269 Grade X6NiCrTiMoVB25-15-2 solution heat-treated and precipitation hardened (+AT+P)

Want to keep this datasheet? Save it now in your required format

Description

High-temperature hardenable special grade with high thermal resistance qualities up to 700 °C and scaling resistance up to 750 °C Application for gas turbine and power unit components, such as wheels, discs, shafts, bolts, screws, intermediate rings, fittings and casings. Further application for mounting elements at increased temperatures.

Related Standards

Equivalent Materials

This material data has been provided by WIAM.

All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

Ashby charts

See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Properties

General

PropertyTemperatureValue

Density

20.0 °C

8 g/cm³

Show Material materials with Density of 8 g/cm³

27.0 °C

7.95 g/cm³

Show Material materials with Density of 7.95 g/cm³

Mechanical

PropertyTemperatureValue

Elastic modulus

-269.0 °C

206.7 GPa

Show Material materials with Elastic modulus of 206.7 GPa

-200.0 °C

206.3 GPa

Show Material materials with Elastic modulus of 206.3 GPa

-150.0 °C

204.6 GPa

Show Material materials with Elastic modulus of 204.6 GPa

-100.0 °C

200.9 GPa

Show Material materials with Elastic modulus of 200.9 GPa

-50.0 °C

197.8 GPa

Show Material materials with Elastic modulus of 197.8 GPa

20.0 °C

211 GPa

Show Material materials with Elastic modulus of 211 GPa

27.0 °C

192.5 GPa

Show Material materials with Elastic modulus of 192.5 GPa

100.0 °C

206 GPa

Show Material materials with Elastic modulus of 206 GPa

200.0 °C

200 GPa

Show Material materials with Elastic modulus of 200 GPa

300.0 °C

192 GPa

Show Material materials with Elastic modulus of 192 GPa

400.0 °C

183 GPa

Show Material materials with Elastic modulus of 183 GPa

500.0 °C

173 GPa

Show Material materials with Elastic modulus of 173 GPa

600.0 °C

162 GPa

Show Material materials with Elastic modulus of 162 GPa

Unlock all property charts

Elongation

20.0 °C

15 %

Show Material materials with Elongation of 15 %

Poisson's ratio

-269.0 °C

0.28 [-]

Show Material materials with Poisson's ratio of 0.28 [-]

-200.0 °C

0.28 [-]

Show Material materials with Poisson's ratio of 0.28 [-]

-150.0 °C

0.28 [-]

Show Material materials with Poisson's ratio of 0.28 [-]

-100.0 °C

0.29 [-]

Show Material materials with Poisson's ratio of 0.29 [-]

-50.0 °C

0.29 [-]

Show Material materials with Poisson's ratio of 0.29 [-]

27.0 °C

0.29 [-]

Show Material materials with Poisson's ratio of 0.29 [-]

Unlock all property charts

Shear modulus

-269.0 °C

80.9 GPa

Show Material materials with Shear modulus of 80.9 GPa

-200.0 °C

80.6 GPa

Show Material materials with Shear modulus of 80.6 GPa

-150.0 °C

79.6 GPa

Show Material materials with Shear modulus of 79.6 GPa

-100.0 °C

78.2 GPa

Show Material materials with Shear modulus of 78.2 GPa

-50.0 °C

76.7 GPa

Show Material materials with Shear modulus of 76.7 GPa

27.0 °C

74.4 GPa

Show Material materials with Shear modulus of 74.4 GPa

Unlock all property charts

Tensile strength

20.0 °C

900 - 1150 MPa

Show Material materials with Tensile strength of 900 - 1150 MPa

400.0 °C

720 MPa

Show Material materials with Tensile strength of 720 MPa

450.0 °C

710 MPa

Show Material materials with Tensile strength of 710 MPa

500.0 °C

700 MPa

Show Material materials with Tensile strength of 700 MPa

550.0 °C

690 MPa

Show Material materials with Tensile strength of 690 MPa

600.0 °C

670 MPa

Show Material materials with Tensile strength of 670 MPa

Unlock all property charts

Yield strength Rp0.2

20.0 °C

600 MPa

Show Material materials with Yield strength Rp0.2 of 600 MPa

50.0 °C

592 MPa

Show Material materials with Yield strength Rp0.2 of 592 MPa

100.0 °C

580 MPa

Show Material materials with Yield strength Rp0.2 of 580 MPa

150.0 °C

570 MPa

Show Material materials with Yield strength Rp0.2 of 570 MPa

200.0 °C

560 MPa

Show Material materials with Yield strength Rp0.2 of 560 MPa

250.0 °C

550 MPa

Show Material materials with Yield strength Rp0.2 of 550 MPa

300.0 °C

540 MPa

Show Material materials with Yield strength Rp0.2 of 540 MPa

350.0 °C

530 MPa

Show Material materials with Yield strength Rp0.2 of 530 MPa

400.0 °C

520 MPa

Show Material materials with Yield strength Rp0.2 of 520 MPa

450.0 °C

510 MPa

Show Material materials with Yield strength Rp0.2 of 510 MPa

500.0 °C

490 MPa

Show Material materials with Yield strength Rp0.2 of 490 MPa

550.0 °C

460 MPa

Show Material materials with Yield strength Rp0.2 of 460 MPa

600.0 °C

430 MPa

Show Material materials with Yield strength Rp0.2 of 430 MPa

650.0 °C

380 MPa

Show Material materials with Yield strength Rp0.2 of 380 MPa

Unlock all property charts

Thermal

PropertyTemperatureValue

Coefficient of thermal expansion

100.0 °C

1.7E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.7E-5 1/K

200.0 °C

1.75E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.75E-5 1/K

300.0 °C

1.78E-5 - 1.83E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.78E-5 - 1.83E-5 1/K

400.0 °C

1.8E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.8E-5 1/K

500.0 °C

1.82E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.82E-5 1/K

600.0 °C

1.85E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.85E-5 1/K

Unlock all property charts

Max service temperature, long

0 - 700 °C

Show Material materials with Max service temperature, long of 0 - 700 °C

Chemical properties

PropertyValue

Aluminium

0.35 %

Show Material materials with Aluminium of 0.35 %

Boron

0.003 - 0.01 %

Show Material materials with Boron of 0.003 - 0.01 %

Carbon

0.03 - 0.08 %

Show Material materials with Carbon of 0.03 - 0.08 %

Chromium

13.5 - 16 %

Show Material materials with Chromium of 13.5 - 16 %

Manganese

1 - 2 %

Show Material materials with Manganese of 1 - 2 %

Molybdenum

1 - 1.5 %

Show Material materials with Molybdenum of 1 - 1.5 %

Nickel

24 - 27 %

Show Material materials with Nickel of 24 - 27 %

Phosphorus

0.03 %

Show Material materials with Phosphorus of 0.03 %

Silicon

1 %

Show Material materials with Silicon of 1 %

Sulfur

0.015 %

Show Material materials with Sulfur of 0.015 %

Titanium

1.9 - 2.3 %

Show Material materials with Titanium of 1.9 - 2.3 %

Vanadium

0.1 - 0.5 %

Show Material materials with Vanadium of 0.1 - 0.5 %